C93500 Leaded Bronze 85-5-10, Cast Material Data Sheet

C93500 Leaded Bronze 85-5-10 Material Data Sheet (Cast)

C93500 Cast Bronze Overview

C93500 cast bronze is a cast bronze (UNS C93500), known as leaded bronze 85-5-10. Condition: Cast. This C93500 cast bronze material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C93500 bronze castings from Turkey (Türkiye)? Modulus Metal supplies C93500 bronze castings with in-house CNC machining and inspects them before shipment.

C93500 Designation

Copper Alloy: CuSn5Pb10 (UNS C93500)
UNS numberC93500

C93500 Typical uses

Bearings and bushes to resist corrosion and poor lubrication (plasticity increases with lead content, making them suitable for minor misalignment and for use with soft steel shafts).

C93500 Cast Bronze Composition detail

Al (aluminum)0–0.005%
Cu (copper)80.4–87.7%
Fe (iron)0–0.2%
Ni (nickel)0–1%
P (phosphorus)0–0.05%
Pb (lead)8–10%
S (sulfur)0–0.08%
Sb (antimony)0–0.3%
Si (silicon)0–0.005%
Sn (tin)4.3–6%
Zn (zinc)0–2%

C93500 Physical properties

Density8.91–9.09g/cm3

C93500 Cast Bronze Mechanical properties

Young’s modulus72–74GPa
Specific stiffness7.97–8.25MN.m/kg
Yield strength (elastic limit)60–130MPa
Tensile strength160–230MPa
Specific strength6.67–14.4kN.m/kg
Elongation5–9% strain
Compressive strength60–130MPa
Flexural modulus72–74GPa
Flexural strength (modulus of rupture)60–130MPa
Shear modulus26.6–27.4GPa
Bulk modulus77.8–79.9GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers55–75HV
Hardness – Brinell55–80HB
Elastic stored energy (springs)27.5–104kJ/m3
Fatigue strength at 10^7 cycles90–100MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
67.6–133MPa

C93500 Impact & fracture properties

Fracture toughness76–90.5MPa.m0.5
Toughness (G)79.7–111kJ/m2

C93500 Cast Bronze Thermal properties

Melting point927–1060°C
Maximum service temperature180–190°C
Minimum service temperature-273  °C
Thermal conductivity68–74W/m.°C
Specific heat capacity376–392J/kg.°C
Thermal expansion coefficient18–19µstrain/°C
Thermal shock resistance44.4–96.4°C
Thermal distortion resistance3.65–4.03MW/m
Latent heat of fusion220–240kJ/kg

C93500 Electrical properties

Electrical resistivity11–12µohm.cm
Electrical conductivity14.4–15.7%IACS
Galvanic potential-0.25–-0.17V

C93500 Magnetic properties

Magnetic typeNon-magnetic

C93500 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2820–2870m/s
Mechanical loss coefficient (tan delta)4e-4–0.00111 

C93500 Processing properties

Metal castingExcellent
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed91.4 m/min
WeldabilityUnsuitable

C93500 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Contains lead which lubricates, improving resistance.
Excellent
FlammabilityNon-flammable

C93500 Cast Bronze Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

C93500 Notes

C93500 Cast Bronze Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C93500 Standards with similar compositions

Australia: C93500 to AS 2738
Europe: CB494K to CEN EN 1982, CC494K to CEN EN 1982
International: CuPb9Sn5 to ISO 4382-1
USA: C93500, C93500 to ASTM B271, C93500 to ASTM B30, C93500 to ASTM B505, C93500 to ASTM B584, C93500 to ASTM B763, C93500 to CDA Datasheet, C93500 to SAE J462, UNS C93500
Venezuela: C93500 to COPANT 801
Tradenames: BUNTING NO. 935, WRM 59