CuSn10 (C90700) Tin Bronze, Cast Material Data Sheet

CuSn10 (C90700) Tin Bronze Material Data Sheet (Cast)

CuSn10 C90700 Cast Overview

CuSn10 C90700 cast is a cast bronze (UNS C90700, EN CC480K), known as tin bronze. Condition: Cast. This CuSn10 C90700 cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for C90700 bronze castings from Turkey (Türkiye)? Modulus Metal supplies C90700 bronze castings with in-house CNC machining and inspects them before shipment.

C90700 Designation

CuSn10
UNS numberC90700
EN nameCC480K
ISO nameCuSn10

C90700 Typical uses

General-purpose sand castings.

CuSn10 C90700 Cast Composition detail

Al (aluminum)0–0.005%
Cu (copper)85.8–90%
Fe (iron)0–0.15%
Ni (nickel)0–0.5%
P (phosphorus)0–0.3%
Pb (lead)0–0.5%
S (sulfur)0–0.05%
Sb (antimony)0–0.2%
Si (silicon)0–0.005%
Sn (tin)10–12%
Zn (zinc)0–0.5%

C90700 Physical properties

Density8.8–8.82g/cm3

CuSn10 C90700 Cast Mechanical properties

Young’s modulus78–82GPa
Specific stiffness8.85–9.31MN.m/kg
Yield strength (elastic limit)130–160MPa
Tensile strength230–310MPa
Specific strength14.8–18.2kN.m/kg
Elongation9–20% strain
Compressive strength130–160MPa
Flexural modulus78–82GPa
Flexural strength (modulus of rupture)130–160MPa
Shear modulus28.9–30.3GPa
Bulk modulus84.2–88.6GPa
Poisson’s ratio0.34–0.35 
Shape factor28
Hardness – Vickers70–90HV
Elastic stored energy (springs)107–159kJ/m3
Fatigue strength at 10^7 cycles123–150MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
101–183MPa

C90700 Impact & fracture properties

Fracture toughness61.3–67.9MPa.m0.5
Toughness (G)47–57.7kJ/m2

CuSn10 C90700 Cast Thermal properties

Melting point887–1040°C
Maximum service temperature150–170°C
Minimum service temperature-273  °C
Thermal conductivity58–63W/m.°C
Specific heat capacity376–392J/kg.°C
Thermal expansion coefficient18–19µstrain/°C
Thermal shock resistance87.4–109°C
Thermal distortion resistance3.11–3.43MW/m
Latent heat of fusion220–240kJ/kg

C90700 Electrical properties

Electrical resistivity14.8–16.6µohm.cm
Electrical conductivity10.4–11.6%IACS
Galvanic potential-0.24–-0.16V

C90700 Magnetic properties

Magnetic typeNon-magnetic

C90700 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2980–3050m/s
Mechanical loss coefficient (tan delta)1.56e-4–2.37e-4 

C90700 Processing properties

Metal castingExcellent
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed36.6 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Good

C90700 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuSn10 C90700 Cast Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Slightly susceptible

C90700 Notes

CuSn10 C90700 Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

C90700 Standards with similar compositions

Czech Republic: CuSn10 to CSN 423119
Japan: CAC502A to JIS H5120
South Africa: Cu-Sn10 to SABS 200, Cu-Sn12P to SABS 200
USA: C90700, C90700 to ASTM B427, C90700 to ASTM B505, C90700 to CDA Datasheet, C90700 to SAE J462, C90800, C90800 to ASTM B30, C90800 to ASTM B427, UNS C90250, UNS C90700, UNS C90800
Tradenames: LILY BRAND NO. 8