AISI 201 Stainless steel (Low nickel work hardenable), austenitic, 1/2 hard | Mechanical Properties

AISI 201 1-2 Hard Stainless Steel Machanical Properties Modulus Metal Turkey Turkiye

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding

Mechanical propertiesValues
Young’s modulus 193 – 201 GPa
Specific stiffness * 24.7 – 25.9 MN.m/kg
Yield strength (elastic limit) 760 – 930 MPa
Tensile strength 1.03e3 – 1.21e3 MPa
Specific strength * 97.4 – 119 kN.m/kg
Elongation 10 – 20 % strain
Compressive strength* 760 – 930 MPa
Flexural modulus * 193 – 201 GPa
Flexural strength (modulus of rupture) 760 – 930 MPa
Shear modulus 75 – 80 GPa
Bulk modulus 136 – 149 GPa
Poisson’s ratio 0.265 – 0.275
Shape factor 28
Hardness – Vickers * 302 – 334 HV
Hardness – Rockwell B * 105 – 108 HRB
Hardness – Rockwell C 30 – 34 HRC
Hardness – Brinell * 285 – 317 HB
Elastic stored energy (springs) 2.19e3 – 2.38e3 kJ/m^3
Fatigue strength at 10^7 cycles * 436 – 490 MPa
Fatigue strength model (stress range) * 389 – 550 MPa
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.

AISI 201 Stainless steel (Low nickel work hardenable), austenitic | Designation | Equivalent Grades & Similar Grades  

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding

Designation: AISI 201

UNS numberS20100
US nameASTM TP201, ASTM S20103, ASTM S20100 Class 2, ASTM S20100 Class 1, ASTM S20100, ~ASTM S20153
EN nameX12CrMnNiN17-7-5
EN number1.4372, 1.4371
GB (Chinese) name1Cr17Mn6Ni5N
JIS (Japanese) nameSUS201
CountryEquivalent / Similar Grade
Australia201-2 to AS 1449
China1Cr17Mn6Ni5N to GB 1220, 1Cr17Mn6Ni5N to GB 4237, 1Cr17Mn6Ni5N to GB/T 3280, 1Cr17Mn6Ni5N to GB/T 4239, 1Cr17Mn6Ni5N to GB/T 4356, 1Cr17Mn6Ni5N to GB/T 6725
IndiaTP201 to IS 11714/4, TP201 to IS 11714/5, X10Cr17Mn6Ni4 to IS 1570/5, X10Cr17Mn6Ni4 to IS 6527, X10Cr17Mn6Ni4 to IS 6528, X10Cr17Mn6Ni4N to IS 6603
InternationalX12CrMnNiN17-7-5 to ISO 6931-2
JapanSUS201 to JIS G4303, SUS201 to JIS G4308, SUS201 to JIS G4309
South KoreaSTS 201 to KS D 3706, STS 201-W1 to KS D 3703, STS201 to KS D 3702
UKX12CrMnNiN17-7-5 to BS EN 10088-1, X12CrMnNiN17-7-5 to BS EN 10088-2, X12CrMnNiN17-7-5 to BS EN 10088-3
USA201 to ASTM A473, S20100 Class 1 to ASTM A666, S20100 Class 2 to ASTM A666, S20100 to ASTM A240/A240M, S20100 to ASTM A276, S20100 to ASTM A959, S20100 to SAE J405, TP201 to ASTM A213/A213M, TP201 to ASTM A249/A249M, UNS S20100
Tradenames: ACX 210, ES 201, UNILOY 201
AISI 201 Stainless steel, austenitic Designation Equivalent Grades & Similar Grades Modulus Metal Turkey

AISI 201 Stainless steel (Low nickel work hardenable), austenitic | Chemical Composition

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding

AISI-201-Stainless-Steel-Chemical-Composition-Modulus-Metal-Turkey
Composition detail%
C (carbon) 0 – 0.15 %
Cr (chromium) 16 – 18 %
Fe (iron)* 67.5 – 75 %
Mn (manganese) 5.5 – 7.5 %
N (nitrogen) 0 – 0.25 %
Ni (nickel) 3.5 – 5.5 %
P (phosphorus) 0 – 0.06 %
S (sulfur) 0 – 0.03 %
Si (silicon) 0 – 1 %
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.

AISI 201 Stainless steel (Low nickel work hardenable), austenitic | Weldability

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding

Weldability*Good
Weldability – MIGExcellent
Weldability – plasmaExcellent
Weldability – SAWExcellent
Weldability – TIGExcellent
BrazeabilityFair
*Notes: Preheating and post weld heat treatments may be required

AISI 201L Stainless steel, annealed (Low nickel work hardenable), austenitic | Designation | Equivalent Grades & Similar Grades

AISI 201L Stainless steel, austenitic annealed Designation Equivalent Grades & Similar Grades Modulus Metal Turkey

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding

Designation

AISI 201

UNS number S20103
US name AISI 201
Standards with similar compositions
UK X2CrMnNiN17-7-5 to BS EN 10088-1, X2CrMnNiN17-7-5 to BS EN 10088-2
USA S20103 to ASTM A240/A240M, S20103 to ASTM A666, S20103 to ASTM A959, S20103 to SAE J405, S20153 to SAE J405, UNS S20103, UNS S20153
Tradenames AISI TYPE 201 MODIFIED, ALLEGHENY LUDLUM TYPE 201 COMPOSITION BALANCED, FIRTH-VICKERS F.S.M.1

AISI 201 Stainless steel (Low nickel work hardenable), austenitic, 3/4 hard | Mechanical Properties

AISI 201 3-4 Hard Stainless Steel Machanical Properties Modulus Metal Turkey Turkiye

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding

Mechanical propertiesValues
Young’s modulus 193 – 201 GPa
Specific stiffness * 24.7 – 25.9 MN.m/kg
Yield strength (elastic limit) 930 – 965 MPa
Tensile strength 1.21e3 – 1.28e3 MPa
Specific strength * 119 – 124 kN.m/kg
Elongation 7 – 10 % strain
Compressive strength * 930 – 965 MPa
Flexural modulus * 193 – 201 GPa
Flexural strength (modulus of rupture) 930 – 965 MPa
Shear modulus 75 – 80 GPa
Bulk modulus 136 – 149 GPa
Poisson’s ratio 0.265 – 0.275
Shape factor 24
Hardness – Vickers * 344 – 382 HV
Hardness – Rockwell B * 109 – 111 HRB
Hardness – Rockwell C 35 – 39 HRC
Hardness – Brinell * 326 – 362 HB
Elastic stored energy (springs) 2.35e3 – 2.55e3 kJ/m^3
Fatigue strength at 10^7 cycles * 489 – 509 MPa
Fatigue strength model (stress range) * 469 – 531 MPa
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.

AISI 201 Stainless steel (Low nickel work hardenable), austenitic, Full hard | Mechanical Properties

AISI 201 Full Hard Stainless Steel Machanical Properties Modulus Metal Turkey Turkiye

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding

Mechanical propertiesValues
Young’s modulus 193 – 201 GPa
Specific stiffness * 24.7 – 25.9 MN.m/kg
Yield strength (elastic limit) 965 – 1e3 MPa
Tensile strength 1.28e3 – 1.35e3 MPa
Specific strength * 123 – 129 kN.m/kg
Elongation 5 – 7 % strain
Compressive strength * 965 – 1e3 MPa
Flexural modulus * 193 – 201 GPa
Flexural strength (modulus of rupture) 965 – 1e3 MPa
Shear modulus 75 – 80 GPa
Bulk modulus 136 – 149 GPa
Poisson’s ratio 0.265 – 0.275
Shape factor 23
Hardness – Vickers * 381 – 423 HV
Hardness – Rockwell B * 110 – 114 HRB
Hardness – Rockwell C 38 – 44 HRC
Hardness – Brinell * 361 – 401 HB
Elastic stored energy (springs) 235 – 286 kJ/m^3
Fatigue strength at 10^7 cycles * 508 – 529 MPa
Fatigue strength model (stress range) * 489 – 549 MPa
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.

AISI 201 Stainless steel (Low nickel work hardenable), austenitic, Annealed | Mechanical Properties

AISI 201 Annealed Stainless Steel Machanical Properties Modulus Metal Turkey Turkiye

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding

Mechanical propertiesValues
Young’s modulus 193 – 201 GPa
Specific stiffness 24.7 – 25.9 MN.m/kg
Yield strength (elastic limit) 275 – 350 MPa
Tensile strength 655 – 950 MPa
Specific strength 35.2 – 44.9 kN.m/kg
Elongation 40 – 45 % strain
Compressive strength * 275 – 515 MPa
Flexural modulus * 193 – 201 GPa
Flexural strength (modulus of rupture) 275 – 515 MPa
Shear modulus 75 – 80 GPa
Bulk modulus 136 – 149 GPa
Poisson’s ratio 0.265 – 0.275
Shape factor 59
Hardness – Vickers * 180 – 208 HV
Hardness – Rockwell B 85 – 95 HRB
Hardness – Rockwell C * 4 – 15 HRC
Hardness – Brinell 217 – 245 HB
Elastic stored energy (springs) 194 – 307 kJ/m^3
Fatigue strength at 10^7 cycles * 268 – 386 MPa
Fatigue strength model (stress range) * 221 – 468 MPa
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.

AISI 201L Stainless steel (Low nickel work hardenable), austenitic, annealed | Chemical Composition

AISI 201L Stainless Steel Chemical Composition Modulus Metal Turkey

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding

Composition detail%
C (carbon) 0 – 0.03 %
Cr (chromium) 16 – 18 %
Fe (iron)* 67.9 – 75 %
Mn (manganese) 5.5 – 7.5 %
N (nitrogen) 0 – 0.25 %
Ni (nickel) 3.5 – 5.5 %
P (phosphorus) 0 – 0.045 %
S (sulfur) 0 – 0.03 %
Si (silicon) 0 – 0.75 %
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.

AISI 201LN Stainless steel (Low nickel work hardenable), austenitic, annealed | Chemical Composition

AISI 201LN Stainless Steel Chemical Composition Modulus Metal Turkey

Modulus Metal | Manufacturer Company in TURKEY: Sand Casting | Investment Casting | CNC Machining | Press Bending | Laser Cutting | Welding | Plastics Injection Molding

Composition detailValues
C (carbon) 0 – 0.03 %
Cr (chromium) 16 – 17.5 %
Cu (copper) 0 – 1 %
Fe (iron) * 67.9 – 73.5 %
Mn (manganese) 6.4 – 7.5 %
N (nitrogen) 0.1 – 0.25 %
Ni (nickel) ) 4 – 5 %
P (phosphorus 0 – 0.045 %
S (sulfur) ) 0 – 0.015 %
Si (silicon 0 – 0.75 %
*Values indicated with asterisks (*) are approximate. No guarantee is provided for the precision of this information.