PA66 60% Long Glass Fiber Material Data Sheet

PA66 60% Long Glass Fiber (Polyamide 66) Material Data Sheet

PA66 60% Long Glass Fiber Overview

PA66 60% long glass fiber is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 60% Long Glass Fiber). This PA66 60% long glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 60% Long Glass Fiber Designation

Polyamide (Nylon) (Type 66, 60% Long Glass Fiber)
TradenamesCelstran, LNP Verton, Onforce, Polytron

PA66 60% Long Glass Fiber Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA66 60% Long Glass Fiber Composition detail

Polymer40  %
Glass (fiber)60  %

PA66 60% Long Glass Fiber Physical properties

Density1.65–1.69g/cm3

PA66 60% Long Glass Fiber Mechanical properties

Young’s modulus12.5–15.5GPa
Specific stiffness7.48–9.29MN.m/kg
Yield strength (elastic limit)169–211MPa
Tensile strength171–209MPa
Specific strength101–126kN.m/kg
Elongation1.64–2.36% strain
Elongation at yield1.38–2.62% strain
Compressive modulus13.3–14.7GPa
Compressive strength217–239MPa
Flexural modulus13.3–16GPa
Flexural strength (modulus of rupture)290–354MPa
Shear modulus5.13–5.39GPa
Shear strength103–125MPa
Bulk modulus13.1–14.5GPa
Poisson’s ratio0.318–0.331 
Shape factor6.69
Hardness – Vickers54–60HV
Hardness – Rockwell M184–204 
Hardness – Rockwell R184–204 
Hardness – Shore D98–102 
Elastic stored energy (springs)1020–1610kJ/m3
Fatigue strength at 10^7 cycles72.2–79.8MPa

PA66 60% Long Glass Fiber Impact & fracture properties

Fracture toughness5.21–5.76MPa.m0.5
Toughness (G)1.87–2.49kJ/m2
Impact strength, notched 23 °C27.2–52.8kJ/m2
Impact strength, notched -30 °C28.4–61.7kJ/m2
Impact strength, unnotched 23 °C77–113kJ/m2
Impact strength, unnotched -30 °C72–108kJ/m2

PA66 60% Long Glass Fiber Thermal properties

Melting point250–271°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa263–317°C
Heat deflection temperature 1.8MPa237–290°C
Maximum service temperature90–130°C
Minimum service temperature-81–-71°C
Thermal conductivity0.53–0.57W/m.°C
Specific heat capacity1210–1260J/kg.°C
Thermal expansion coefficient19.8–20.2µstrain/°C
Thermal shock resistance583–789°C
Thermal distortion resistance0.0265–0.0285MW/m

PA66 60% Long Glass Fiber Electrical properties

Electrical resistivity2e17–5e18µohm.cm
Electrical conductivity3.45e-17–8.62e-16%IACS
Dielectric constant (relative permittivity)10.2–14.3 
Dissipation factor (dielectric loss tangent)0.0857–0.226 
Dielectric strength (dielectric breakdown)39.2–66.8MV/m
Comparative tracking index475–525V

PA66 60% Long Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PA66 60% Long Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2730–3050m/s
Mechanical loss coefficient (tan delta)0.00656–0.00725 

PA66 60% Long Glass Fiber Absorption & permeability

Water absorption @ 24 hrs0.25–0.4%
Water absorption @ sat2.8–3.7%
Humidity absorption @ sat0.81–1.1%

PA66 60% Long Glass Fiber Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 0.6 %
Melt temperature239 – 316 °C
Mold temperature40 – 60 °C
Molding pressure range68.8 – 138 MPa

PA66 60% Long Glass Fiber Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySlow-burning