Home » PA (Polyamide / Nylon) » PA66 (Polyamide 66 / Nylon 66) » PA66 Glass Filled Grades » PA66 20-25% Glass Fiber Flame Retarded Material Data Sheet
PA66 20-25% Glass Fiber Flame Retarded (Polyamide 66) Material Data Sheet
PA66 20-25% Glass Fiber Flame Retarded Overview
PA66 20-25% glass fiber flame retarded is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 20-25% Glass Fiber, Flame Retarded). This PA66 20-25% glass fiber flame retarded material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.
PA66 20-25% Glass Fiber Flame Retarded Designation
Polyamide (Nylon) (Type 66, 20-25% Glass Fiber, Flame Retarded) Tradenames Bergamid, Frianyl, Hifill, LNP Thermocomp
PA66 20-25% Glass Fiber Flame Retarded Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA66 20-25% Glass Fiber Flame Retarded Composition detail
Polymer 60 – 75 % Flame retardant 5 – 15 % Glass (fiber) 20 – 25 %
PA66 20-25% Glass Fiber Flame Retarded Physical properties
PA66 20-25% Glass Fiber Flame Retarded Mechanical properties
Young’s modulus 5.84 – 7.28 GPa Specific stiffness 4.01 – 5.01 MN.m/kg Yield strength (elastic limit) 93.5 – 117 MPa Tensile strength 91.4 – 112 MPa Specific strength 64.2 – 80.4 kN.m/kg Elongation 3.29 – 4.73 % strain Elongation at yield 2.63 – 4.99 % strain Compressive modulus 6.23 – 6.89 GPa Compressive strength 116 – 128 MPa Flexural modulus 3.82 – 4.58 GPa Flexural strength (modulus of rupture) 156 – 191 MPa Shear modulus 2.35 – 2.47 GPa Shear strength 54.8 – 67 MPa Bulk modulus 7.42 – 8.2 GPa Poisson’s ratio 0.34 – 0.36 Shape factor 6 Hardness – Vickers 30 – 33 HV Hardness – Rockwell M 146 – 161 Hardness – Rockwell R 146 – 161 Hardness – Brinell 118 – 148 HB Hardness – Shore D 89 – 93 Elastic stored energy (springs) 663 – 1060 kJ/m3 Fatigue strength at 10^7 cycles 38.6 – 42.6 MPa
PA66 20-25% Glass Fiber Flame Retarded Impact & fracture properties
Fracture toughness 4.47 – 4.94 MPa.m0.5 Toughness (G) 2.93 – 3.91 kJ/m2 Impact strength, notched 23 °C 9.03 – 17.5 kJ/m2 Impact strength, notched -30 °C 5.26 – 11.4 kJ/m2 Impact strength, unnotched 23 °C 50.6 – 74.3 kJ/m2 Impact strength, unnotched -30 °C 47.2 – 70.8 kJ/m2
PA66 20-25% Glass Fiber Flame Retarded Thermal properties
Melting point 260 – 265 °C Glass temperature 54 – 66 °C Heat deflection temperature 0.45MPa 225 – 276 °C Heat deflection temperature 1.8MPa 225 – 276 °C Maximum service temperature 90 – 130 °C Minimum service temperature -81 – -71 °C Thermal conductivity 0.436 – 0.453 W/m.°C Specific heat capacity 1380 – 1430 J/kg.°C Thermal expansion coefficient 88.2 – 91.8 µstrain/°C Thermal shock resistance 153 – 208 °C Thermal distortion resistance 0.00481 – 0.00508 MW/m
PA66 20-25% Glass Fiber Flame Retarded Electrical properties
Electrical resistivity 3.54e19 – 8.86e20 µohm.cm Electrical conductivity 1.95e-19 – 4.87e-18 %IACS Dielectric constant (relative permittivity) 3.98 – 5.62 Dissipation factor (dielectric loss tangent) 0.0066 – 0.0174 Dielectric strength (dielectric breakdown) 29.2 – 49.7 MV/m Comparative tracking index 325 – 600 V
PA66 20-25% Glass Fiber Flame Retarded Magnetic properties
Magnetic type Non-magnetic
PA66 20-25% Glass Fiber Flame Retarded Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 2000 – 2240 m/s Mechanical loss coefficient (tan delta) 0.0123 – 0.0136
PA66 20-25% Glass Fiber Flame Retarded Absorption & permeability
Water absorption @ 24 hrs 0.46 – 0.75 % Water absorption @ sat 4.1 – 5.4 % Humidity absorption @ sat 1.1 – 1.5 %
PA66 20-25% Glass Fiber Flame Retarded Processing properties
Polymer injection molding Limited use Polymer extrusion Limited use Polymer thermoforming Limited use Linear mold shrinkage 0.4 – 0.5 % Melt temperature 212 – 293 °C Mold temperature 40 – 60 °C Molding pressure range 68.8 – 138 MPa
PA66 20-25% Glass Fiber Flame Retarded Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Unacceptable Strong acids Unacceptable Weak alkalis Acceptable Strong alkalis Acceptable Organic solvents Excellent Oxidation at 500C Unacceptable UV radiation (sunlight) Poor Flammability Self-extinguishing