PA66 30-35% Glass Fiber Toughened Material Data Sheet

PA66 30-35% Glass Fiber Toughened (Polyamide 66) Material Data Sheet

PA66 30-35% Glass Fiber Toughened Overview

PA66 30-35% glass fiber toughened is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 30-35% Glass Fiber, Toughened). This PA66 30-35% glass fiber toughened material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 30-35% Glass Fiber Toughened Designation

Polyamide (Nylon) (Type 66, 30-35% Glass Fiber, Toughened)
TradenamesAltech, Mapex, Plustek, Schulamid, Terez, Ultramid, Wellamid

PA66 30-35% Glass Fiber Toughened Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA66 30-35% Glass Fiber Toughened Composition detail

Polymer50–67%
Impact modifier3–15%
Glass (fiber)30–35%

PA66 30-35% Glass Fiber Toughened Physical properties

Density1.27–1.29g/cm3

PA66 30-35% Glass Fiber Toughened Mechanical properties

Young’s modulus5.45–6.8GPa
Specific stiffness4.26–5.31MN.m/kg
Yield strength (elastic limit)93.5–117MPa
Tensile strength97.9–120MPa
Specific strength73–91.4kN.m/kg
Elongation6.56–9.44% strain
Elongation at yield5.52–10.5% strain
Compressive modulus5.82–6.43GPa
Compressive strength124–137MPa
Flexural modulus4.68–5.6GPa
Flexural strength (modulus of rupture)120–147MPa
Shear modulus2.2–2.31GPa
Shear strength58.7–71.8MPa
Bulk modulus6.93–7.66GPa
Poisson’s ratio0.34–0.36 
Shape factor5.79
Hardness – Vickers30–33HV
Hardness – Rockwell M151–167 
Hardness – Rockwell R151–167 
Hardness – Brinell120–150HB
Hardness – Shore D91–94 
Elastic stored energy (springs)711–1140kJ/m3
Fatigue strength at 10^7 cycles41.3–45.7MPa

PA66 30-35% Glass Fiber Toughened Impact & fracture properties

Fracture toughness4.41–4.88MPa.m0.5
Toughness (G)3.06–4.09kJ/m2
Impact strength, notched 23 °C17.2–33.3kJ/m2
Impact strength, notched -30 °C7.75–16.9kJ/m2
Impact strength, unnotched 23 °C80–118kJ/m2
Impact strength, unnotched -30 °C76–114kJ/m2

PA66 30-35% Glass Fiber Toughened Thermal properties

Melting point256–265°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa249–257°C
Heat deflection temperature 1.8MPa230–243°C
Maximum service temperature57–77°C
Minimum service temperature-81–-71°C
Thermal conductivity0.399–0.415W/m.°C
Specific heat capacity1480–1540J/kg.°C
Thermal expansion coefficient76–79µstrain/°C
Thermal shock resistance190–259°C
Thermal distortion resistance0.00511–0.0054MW/m

PA66 30-35% Glass Fiber Toughened Electrical properties

Electrical resistivity2e17–5e18µohm.cm
Electrical conductivity3.45e-17–8.62e-16%IACS
Dielectric constant (relative permittivity)7.72–10.9 
Dissipation factor (dielectric loss tangent)0.033–0.087 
Dielectric strength (dielectric breakdown)55.5–94.5MV/m
Comparative tracking index500–650V

PA66 30-35% Glass Fiber Toughened Magnetic properties

Magnetic typeNon-magnetic

PA66 30-35% Glass Fiber Toughened Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2060–2310m/s
Mechanical loss coefficient (tan delta)0.0111–0.0123 

PA66 30-35% Glass Fiber Toughened Absorption & permeability

Water absorption @ 24 hrs0.47–0.76%
Water absorption @ sat4.2–5.6%
Humidity absorption @ sat1.2–1.7%

PA66 30-35% Glass Fiber Toughened Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.25 – 0.45 %
Melt temperature225 – 302 °C
Mold temperature40 – 60 °C
Molding pressure range68.8 – 138 MPa

PA66 30-35% Glass Fiber Toughened Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySlow-burning