PA66 10% Glass Fiber Lubricated Material Data Sheet

PA66 10% Glass Fiber Lubricated (Polyamide 66) Material Data Sheet

PA66 10% Glass Fiber Lubricated Overview

PA66 10% glass fiber lubricated is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 10% Glass Fiber, Lubricated, 5-20% PTFE). This PA66 10% glass fiber lubricated material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 10% Glass Fiber Lubricated Designation

Polyamide (Nylon) (Type 66, 10% Glass Fiber, Lubricated, 5-20% PTFE)
TradenamesHifill, LNP Lubricomp, Lubriblend, Plaslube

PA66 10% Glass Fiber Lubricated Typical uses

Automotive under the hood, bearings, business equipment, chemical process, gears, general purpose, parts (engineering), switches, textile applications

PA66 10% Glass Fiber Lubricated Composition detail

Polymer70–85%
PTFE (lubricant)5–20%
Glass (fiber)10  %

PA66 10% Glass Fiber Lubricated Physical properties

Density1.23–1.34g/cm3

PA66 10% Glass Fiber Lubricated Mechanical properties

Young’s modulus4.14–5.64GPa
Specific stiffness3.21–4.41MN.m/kg
Yield strength (elastic limit)77.3–90.1MPa
Tensile strength93.1–107MPa
Specific strength59.6–70.9kN.m/kg
Elongation2.5–4.2% strain
Elongation at yield2.5–3.5% strain
Compressive modulus2.83–2.97GPa
Compressive strength86.2–100MPa
Flexural modulus4.14–5.3GPa
Flexural strength (modulus of rupture)131–165MPa
Shear modulus1.72–1.81GPa
Shear strength55.4–64.7MPa
Bulk modulus4.71–4.95GPa
Poisson’s ratio0.364–0.379 
Shape factor5.8
Hardness – Vickers23–26HV
Hardness – Rockwell R119
Hardness – Shore D83–91 
Elastic stored energy (springs)585–887kJ/m3
Fatigue strength at 10^7 cycles32.1–37.4MPa

PA66 10% Glass Fiber Lubricated Impact & fracture properties

Fracture toughness4.69–5.67MPa.m0.5
Toughness (G)4.36–6.93kJ/m2
Impact strength, notched 23 °C4–5.9kJ/m2
Impact strength, notched -30 °C4.37–5.29kJ/m2
Impact strength, unnotched 23 °C28–48.2kJ/m2

PA66 10% Glass Fiber Lubricated Thermal properties

Melting point237–277°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa238–260°C
Heat deflection temperature 1.8MPa224–246°C
Vicat softening point245  °C
Maximum service temperature107–127°C
Minimum service temperature-81–-71°C
Thermal conductivity0.35  W/m.°C
Specific heat capacity1510–1570J/kg.°C
Thermal expansion coefficient44.2–74.9µstrain/°C
Thermal shock resistance222–406°C
Thermal distortion resistance0.00467–0.00792MW/m

PA66 10% Glass Fiber Lubricated Electrical properties

Electrical resistivity1e20  µohm.cm
Electrical conductivity1.72e-18 %IACS
Dielectric constant (relative permittivity)3.7
Dissipation factor (dielectric loss tangent)0.018
Dielectric strength (dielectric breakdown)20  MV/m
Comparative tracking index450–550V

PA66 10% Glass Fiber Lubricated Magnetic properties

Magnetic typeNon-magnetic

PA66 10% Glass Fiber Lubricated Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1790–2110m/s
Mechanical loss coefficient (tan delta)0.0105–0.0138 

PA66 10% Glass Fiber Lubricated Absorption & permeability

Water absorption @ 24 hrs0.64–0.9%
Water absorption @ sat4–4.7%
Humidity absorption @ sat0.97  %

PA66 10% Glass Fiber Lubricated Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.5 – 1.4 %
Melt temperature275 – 304 °C
Mold temperature65.6 – 110 °C
Molding pressure range68.9 – 138 MPa

PA66 10% Glass Fiber Lubricated Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySlow-burning