PA66 30% Long Glass Fiber (Polyamide 66) Material Data Sheet
PA66 30% Long Glass Fiber Overview
PA66 30% long glass fiber is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 30% Long Glass Fiber). This PA66 30% long glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.
PA66 30% Long Glass Fiber Designation
Polyamide (Nylon) (Type 66, 30% Long Glass Fiber)
Tradenames
Ashlene, Celstran, Complet, Polytron
PA66 30% Long Glass Fiber Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA66 30% Long Glass Fiber Composition detail
Polymer
70
%
Glass (fiber)
30
%
PA66 30% Long Glass Fiber Physical properties
Density
1.36
–
1.39
g/cm3
PA66 30% Long Glass Fiber Mechanical properties
Young’s modulus
5.9
–
7.36
GPa
Specific stiffness
4.29
–
5.36
MN.m/kg
Yield strength (elastic limit)
112
–
139
MPa
Tensile strength
113
–
138
MPa
Specific strength
81.4
–
101
kN.m/kg
Elongation
3.03
–
4.36
% strain
Elongation at yield
2.55
–
4.84
% strain
Compressive modulus
6.3
–
6.96
GPa
Compressive strength
143
–
158
MPa
Flexural modulus
5.95
–
7.13
GPa
Flexural strength (modulus of rupture)
164
–
201
MPa
Shear modulus
2.38
–
2.5
GPa
Shear strength
67.7
–
82.8
MPa
Bulk modulus
7.5
–
8.29
GPa
Poisson’s ratio
0.34
–
0.36
Shape factor
5.47
Hardness – Vickers
36
–
40
HV
Hardness – Rockwell M
162
–
179
Hardness – Rockwell R
162
–
179
Hardness – Shore D
93
–
97
Elastic stored energy (springs)
940
–
1480
kJ/m3
Fatigue strength at 10^7 cycles
47.7
–
52.7
MPa
PA66 30% Long Glass Fiber Impact & fracture properties
Fracture toughness
4.48
–
4.95
MPa.m0.5
Toughness (G)
2.91
–
3.89
kJ/m2
Impact strength, notched 23 °C
15.2
–
29.5
kJ/m2
Impact strength, notched -30 °C
10.8
–
23.5
kJ/m2
Impact strength, unnotched 23 °C
68.7
–
101
kJ/m2
PA66 30% Long Glass Fiber Thermal properties
Melting point
260
–
265
°C
Glass temperature
54
–
66
°C
Heat deflection temperature 0.45MPa
237
–
290
°C
Heat deflection temperature 1.8MPa
252
–
257
°C
Maximum service temperature
90
–
130
°C
Minimum service temperature
-81
–
-71
°C
Thermal conductivity
0.436
–
0.453
W/m.°C
Specific heat capacity
1350
–
1450
J/kg.°C
Thermal expansion coefficient
41.2
–
43
µstrain/°C
Thermal shock resistance
386
–
524
°C
Thermal distortion resistance
0.0102
–
0.0109
MW/m
PA66 30% Long Glass Fiber Electrical properties
Electrical resistivity
2e17
–
5e18
µohm.cm
Electrical conductivity
3.45e-17
–
8.62e-16
%IACS
Dielectric constant (relative permittivity)
8.56
–
12.1
Dissipation factor (dielectric loss tangent)
0.136
–
0.358
Dielectric strength (dielectric breakdown)
27.8
–
47.3
MV/m
Comparative tracking index
475
–
525
V
PA66 30% Long Glass Fiber Magnetic properties
Magnetic type
Non-magnetic
PA66 30% Long Glass Fiber Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2070
–
2320
m/s
Mechanical loss coefficient (tan delta)
0.00983
–
0.0109
PA66 30% Long Glass Fiber Absorption & permeability