PA66 40% Glass Fiber Lubricated Material Data Sheet

PA66 40% Glass Fiber Lubricated (Polyamide 66) Material Data Sheet

PA66 40% Glass Fiber Lubricated Overview

PA66 40% glass fiber lubricated is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 40% Glass Fiber, Lubricated, 5-20% PTFE). This PA66 40% glass fiber lubricated material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 40% Glass Fiber Lubricated Designation

Polyamide (Nylon) (Type 66, 40% Glass Fiber, Lubricated, 5-20% PTFE)
TradenamesEplamid, Latilub, LNP Lubricomp, Luvocom, Nypol, RTP, Tribocomp, Vitamide

PA66 40% Glass Fiber Lubricated Typical uses

Automotive applications, bearings, business equipment, gears, parts (engineering), switches, textile applications

PA66 40% Glass Fiber Lubricated Composition detail

Polymer40–55%
PTFE (lubricant)5–20%
Glass (fiber)40  %

PA66 40% Glass Fiber Lubricated Physical properties

Density1.46–1.61g/cm3

PA66 40% Glass Fiber Lubricated Mechanical properties

Young’s modulus10.3–13.4GPa
Specific stiffness6.68–8.81MN.m/kg
Yield strength (elastic limit)139–162MPa
Tensile strength168–204MPa
Specific strength89.3–107kN.m/kg
Elongation2–3% strain
Elongation at yield2–4% strain
Compressive modulus6.88–7.23GPa
Compressive strength124–138MPa
Flexural modulus8.96–12.4GPa
Flexural strength (modulus of rupture)252–294MPa
Shear modulus4.25–4.47GPa
Shear strength103–120MPa
Bulk modulus11.5–12GPa
Poisson’s ratio0.34–0.354 
Shape factor7
Hardness – Vickers42–46HV
Hardness – Rockwell R120–122 
Hardness – Shore D92–102 
Elastic stored energy (springs)785–1160kJ/m3
Fatigue strength at 10^7 cycles50.9–59.4MPa

PA66 40% Glass Fiber Lubricated Impact & fracture properties

Fracture toughness7.21–8.73MPa.m0.5
Toughness (G)4.31–6.67kJ/m2
Impact strength, notched 23 °C11.6–15.8kJ/m2
Impact strength, notched -30 °C11.1–13.4kJ/m2
Impact strength, unnotched 23 °C50.6–126kJ/m2
Impact strength, unnotched -30 °C50  kJ/m2

PA66 40% Glass Fiber Lubricated Thermal properties

Melting point250–265°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa245–270°C
Heat deflection temperature 1.8MPa240–260°C
Vicat softening point250  °C
Maximum service temperature107–127°C
Minimum service temperature-81–-71°C
Thermal conductivity0.52  W/m.°C
Specific heat capacity1480–1530J/kg.°C
Thermal expansion coefficient24–36µstrain/°C
Thermal shock resistance339–553°C
Thermal distortion resistance0.0144–0.0217MW/m

PA66 40% Glass Fiber Lubricated Electrical properties

Electrical resistivity1e20–1e22µohm.cm
Electrical conductivity1.72e-20–1.72e-18%IACS
Dielectric constant (relative permittivity)3.8
Dissipation factor (dielectric loss tangent)0.015
Dielectric strength (dielectric breakdown)20–37MV/m
Comparative tracking index450–500V

PA66 40% Glass Fiber Lubricated Magnetic properties

Magnetic typeNon-magnetic

PA66 40% Glass Fiber Lubricated Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2580–2980m/s
Mechanical loss coefficient (tan delta)0.00671–0.00888 

PA66 40% Glass Fiber Lubricated Absorption & permeability

Water absorption @ 24 hrs0.5–1%
Water absorption @ sat4.1  %
Humidity absorption @ sat0.86–1.2%

PA66 40% Glass Fiber Lubricated Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 0.4 %
Melt temperature260 – 304 °C
Mold temperature65.6 – 120 °C
Molding pressure range68.9 – 138 MPa

PA66 40% Glass Fiber Lubricated Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySlow-burning