PA66 60% Glass Fiber Material Data Sheet

PA66 60% Glass Fiber (Polyamide 66) Material Data Sheet

PA66 60% Glass Fiber Overview

PA66 60% glass fiber is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 60% Glass Fiber). This PA66 60% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 60% Glass Fiber Designation

Polyamide (Nylon) (Type 66, 60% Glass Fiber)
TradenamesAkromid, Altech, Amilan, Aquaforce, Ashlene, Deslon, Latamid, Latigloss, Leona, Lumid, Maxamid, Nycal, Nylaforce, Nylene, Nymax, Opnyl, Plastron, Polytron, RTP, Strator, Technyl Star, Tecomid, Tekamid, Terez, Ultramid, Unitika, VLF

PA66 60% Glass Fiber Typical uses

Automotive exterior parts, construction applications, consumer applications, general purpose, industrial applications, metal replacement

PA66 60% Glass Fiber Composition detail

Polymer40  %
Glass (fiber)60  %

PA66 60% Glass Fiber Physical properties

Density1.68–1.72g/cm3

PA66 60% Glass Fiber Mechanical properties

Young’s modulus15.2–22.5GPa
Specific stiffness8.94–13.2MN.m/kg
Yield strength (elastic limit)220–250MPa
Tensile strength200–275MPa
Specific strength129–147kN.m/kg
Elongation1.5–3.5% strain
Compressive modulus10.8–11.4GPa
Compressive strength207  MPa
Flexural modulus14.9–20GPa
Flexural strength (modulus of rupture)314–400MPa
Shear modulus6.81–7.16GPa
Shear strength130–152MPa
Bulk modulus18–19GPa
Poisson’s ratio0.318–0.331 
Shape factor7
Hardness – Vickers52–58HV
Hardness – Rockwell M88–98 
Hardness – Rockwell R117–130 
Hardness – Shore D100–110 
Hardness – Shore A95
Elastic stored energy (springs)1190–1860kJ/m3
Fatigue strength at 10^7 cycles62–72.3MPa

PA66 60% Glass Fiber Impact & fracture properties

Fracture toughness11.3–13.7MPa.m0.5
Toughness (G)6.43–10.8kJ/m2
Impact strength, notched 23 °C13.5–22kJ/m2
Impact strength, notched -30 °C10–12kJ/m2
Impact strength, unnotched 23 °C58.5–110kJ/m2
Impact strength, unnotched -30 °C85  kJ/m2

PA66 60% Glass Fiber Thermal properties

Melting point254–262°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa249–265°C
Heat deflection temperature 1.8MPa210–260°C
Vicat softening point240–255°C
Maximum service temperature135  °C
Minimum service temperature-81–-71°C
Thermal conductivity0.4–0.55W/m.°C
Specific heat capacity1500  J/kg.°C
Thermal expansion coefficient20–27µstrain/°C
Thermal shock resistance427–698°C
Thermal distortion resistance0.0163–0.025MW/m

PA66 60% Glass Fiber Electrical properties

Electrical resistivity1e20–1e22µohm.cm
Electrical conductivity1.72e-20–1.72e-18%IACS
Dielectric constant (relative permittivity)3.9–4 
Dissipation factor (dielectric loss tangent)0.014
Dielectric strength (dielectric breakdown)20–25MV/m
Comparative tracking index475–600V

PA66 60% Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PA66 60% Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2980–3660m/s
Mechanical loss coefficient (tan delta)0.00535–0.00708 

PA66 60% Glass Fiber Absorption & permeability

Water absorption @ 24 hrs0.36–0.52%
Water absorption @ sat2.8–3.4%
Humidity absorption @ sat0.7–1%

PA66 60% Glass Fiber Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 0.379 %
Melt temperature230 – 320 °C
Mold temperature60 – 130 °C
Molding pressure range82.7 – 138 MPa

PA66 60% Glass Fiber Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySlow-burning