PA66 50% Long Glass Fiber Lubricated Material Data Sheet

PA66 50% Long Glass Fiber Lubricated (Polyamide 66) Material Data Sheet

PA66 50% Long Glass Fiber Lubricated Overview

PA66 50% long glass fiber lubricated is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 50% Long Glass Fiber, Lubricated, 5-20% PTFE). This PA66 50% long glass fiber lubricated material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 50% Long Glass Fiber Lubricated Designation

Polyamide (Nylon) (Type 66, 50% Long Glass Fiber, Lubricated, 5-20% PTFE)
TradenamesHifill, LNP Verton

PA66 50% Long Glass Fiber Lubricated Typical uses

Automotive applications, structural parts

PA66 50% Long Glass Fiber Lubricated Composition detail

Polymer30–45%
PTFE (lubricant)5–20%
Glass (fiber)50  %

PA66 50% Long Glass Fiber Lubricated Physical properties

Density1.59–1.65g/cm3

PA66 50% Long Glass Fiber Lubricated Mechanical properties

Young’s modulus14.9–15.6GPa
Specific stiffness9.13–9.71MN.m/kg
Yield strength (elastic limit)188–219MPa
Tensile strength231–276MPa
Specific strength116–135kN.m/kg
Elongation1.5–2.3% strain
Compressive modulus8.93–9.38GPa
Compressive strength281–327MPa
Flexural modulus14.1–16.5GPa
Flexural strength (modulus of rupture)345–362MPa
Shear modulus5.57–5.85GPa
Shear strength140–164MPa
Bulk modulus14.9–15.6GPa
Poisson’s ratio0.33–0.343 
Shape factor6.8
Hardness – Vickers56–62HV
Hardness – Rockwell R121
Hardness – Shore D97–107 
Elastic stored energy (springs)1160–1560kJ/m3
Fatigue strength at 10^7 cycles66–77MPa

PA66 50% Long Glass Fiber Lubricated Impact & fracture properties

Fracture toughness9.97–12.1MPa.m0.5
Toughness (G)6.57–9.48kJ/m2
Impact strength, notched 23 °C29–44kJ/m2
Impact strength, notched -30 °C28.2–34.1kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2

PA66 50% Long Glass Fiber Lubricated Thermal properties

Melting point237–277°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa260–265°C
Heat deflection temperature 1.8MPa258–260°C
Vicat softening point240–255°C
Maximum service temperature107–127°C
Minimum service temperature-81–-71°C
Thermal conductivity0.519–0.54W/m.°C
Specific heat capacity1280–1330J/kg.°C
Thermal expansion coefficient27  µstrain/°C
Thermal shock resistance454–533°C
Thermal distortion resistance0.0192–0.02MW/m

PA66 50% Long Glass Fiber Lubricated Electrical properties

Electrical resistivity1e21  µohm.cm
Electrical conductivity1.72e-19 %IACS
Dielectric constant (relative permittivity)9.63–13.6 
Dielectric strength (dielectric breakdown)20  MV/m
Comparative tracking index475–600V

PA66 50% Long Glass Fiber Lubricated Magnetic properties

Magnetic typeNon-magnetic

PA66 50% Long Glass Fiber Lubricated Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3020–3120m/s
Mechanical loss coefficient (tan delta)0.00589–0.00779 

PA66 50% Long Glass Fiber Lubricated Absorption & permeability

Water absorption @ 24 hrs0.35  %
Water absorption @ sat3.54–4.1%
Humidity absorption @ sat1.1–1.4%

PA66 50% Long Glass Fiber Lubricated Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.3 %
Melt temperature282 – 304 °C
Mold temperature54.4 – 110 °C
Molding pressure range69 – 138 MPa

PA66 50% Long Glass Fiber Lubricated Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySlow-burning