PA66 50% Long Glass Fiber Material Data Sheet

PA66 50% Long Glass Fiber (Polyamide 66) Material Data Sheet

PA66 50% Long Glass Fiber Overview

PA66 50% long glass fiber is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 50% Long Glass Fiber). This PA66 50% long glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 50% Long Glass Fiber Designation

Polyamide (Nylon) (Type 66, 50% Long Glass Fiber)
TradenamesCelstran, LNP Verton, Onforce, Polytron, Strator, Witcom

PA66 50% Long Glass Fiber Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA66 50% Long Glass Fiber Composition detail

Polymer50  %
Glass (fiber)50  %

PA66 50% Long Glass Fiber Physical properties

Density1.55–1.58g/cm3

PA66 50% Long Glass Fiber Mechanical properties

Young’s modulus10.5–13.1GPa
Specific stiffness6.71–8.37MN.m/kg
Yield strength (elastic limit)156–194MPa
Tensile strength158–193MPa
Specific strength99.6–124kN.m/kg
Elongation1.87–2.69% strain
Elongation at yield1.57–2.99% strain
Compressive modulus11.2–12.4GPa
Compressive strength200–221MPa
Flexural modulus9.93–11.9GPa
Flexural strength (modulus of rupture)274–335MPa
Shear modulus4.28–4.5GPa
Shear strength94.5–116MPa
Bulk modulus11.9–13.1GPa
Poisson’s ratio0.33–0.343 
Shape factor6.32
Hardness – Vickers50–55HV
Hardness – Rockwell M184–204 
Hardness – Rockwell R184–204 
Hardness – Shore D98–102 
Elastic stored energy (springs)1030–1620kJ/m3
Fatigue strength at 10^7 cycles66.5–73.5MPa

PA66 50% Long Glass Fiber Impact & fracture properties

Fracture toughness5.03–5.56MPa.m0.5
Toughness (G)2.06–2.76kJ/m2
Impact strength, notched 23 °C22.4–43.6kJ/m2
Impact strength, notched -30 °C22.3–48.4kJ/m2
Impact strength, unnotched 23 °C58.3–85.7kJ/m2
Impact strength, unnotched -30 °C53.9–80.8kJ/m2

PA66 50% Long Glass Fiber Thermal properties

Melting point260–265°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa260–314°C
Heat deflection temperature 1.8MPa235–287°C
Maximum service temperature90–130°C
Minimum service temperature-81–-71°C
Thermal conductivity0.51–0.55W/m.°C
Specific heat capacity1280–1330J/kg.°C
Thermal expansion coefficient22.2–22.7µstrain/°C
Thermal shock resistance567–769°C
Thermal distortion resistance0.0227–0.0245MW/m

PA66 50% Long Glass Fiber Electrical properties

Electrical resistivity2e17–5e18µohm.cm
Electrical conductivity3.45e-17–8.62e-16%IACS
Dielectric constant (relative permittivity)9.63–13.6 
Dissipation factor (dielectric loss tangent)0.101–0.265 
Dielectric strength (dielectric breakdown)35.8–60.9MV/m
Comparative tracking index475–525V

PA66 50% Long Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PA66 50% Long Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2590–2900m/s
Mechanical loss coefficient (tan delta)0.00761–0.00841 

PA66 50% Long Glass Fiber Absorption & permeability

Water absorption @ 24 hrs0.46–0.74%
Water absorption @ sat3.8–5%
Humidity absorption @ sat0.85–1.2%

PA66 50% Long Glass Fiber Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 0.7 %
Melt temperature231 – 304 °C
Mold temperature40 – 60 °C
Molding pressure range68.8 – 138 MPa

PA66 50% Long Glass Fiber Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySlow-burning