PA66 40% Long Glass Fiber (Polyamide 66) Material Data Sheet
PA66 40% Long Glass Fiber Overview
PA66 40% long glass fiber is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 40% Long Glass Fiber). This PA66 40% long glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.
PA66 40% Long Glass Fiber Designation
Polyamide (Nylon) (Type 66, 40% Long Glass Fiber)
Tradenames
Celstran, LNP Verton, Onforce, Polytron
PA66 40% Long Glass Fiber Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA66 40% Long Glass Fiber Composition detail
Polymer
60
%
Glass (fiber)
40
%
PA66 40% Long Glass Fiber Physical properties
Density
1.45
–
1.47
g/cm3
PA66 40% Long Glass Fiber Mechanical properties
Young’s modulus
8.9
–
11.1
GPa
Specific stiffness
6.09
–
7.6
MN.m/kg
Yield strength (elastic limit)
142
–
178
MPa
Tensile strength
144
–
176
MPa
Specific strength
97.2
–
122
kN.m/kg
Elongation
1.64
–
2.36
% strain
Elongation at yield
1.38
–
2.62
% strain
Compressive modulus
9.5
–
10.5
GPa
Compressive strength
182
–
202
MPa
Flexural modulus
8.65
–
10.4
GPa
Flexural strength (modulus of rupture)
243
–
297
MPa
Shear modulus
3.6
–
3.79
GPa
Shear strength
86.4
–
106
MPa
Bulk modulus
10.8
–
12
GPa
Poisson’s ratio
0.34
–
0.354
Shape factor
6
Hardness – Vickers
46
–
50
HV
Hardness – Rockwell M
181
–
200
Hardness – Rockwell R
181
–
200
Hardness – Shore D
97
–
101
Elastic stored energy (springs)
1000
–
1610
kJ/m3
Fatigue strength at 10^7 cycles
60.8
–
67.2
MPa
PA66 40% Long Glass Fiber Impact & fracture properties
Fracture toughness
4.87
–
5.38
MPa.m0.5
Toughness (G)
2.28
–
3.04
kJ/m2
Impact strength, notched 23 °C
18.4
–
35.6
kJ/m2
Impact strength, notched -30 °C
23.3
–
50.7
kJ/m2
Impact strength, unnotched 23 °C
55.1
–
80.9
kJ/m2
Impact strength, unnotched -30 °C
52
–
78
kJ/m2
PA66 40% Long Glass Fiber Thermal properties
Melting point
210
–
230
°C
Glass temperature
54
–
66
°C
Heat deflection temperature 0.45MPa
229
–
281
°C
Heat deflection temperature 1.8MPa
229
–
281
°C
Maximum service temperature
90
–
130
°C
Minimum service temperature
-81
–
-71
°C
Thermal conductivity
0.507
–
0.527
W/m.°C
Specific heat capacity
1340
–
1400
J/kg.°C
Thermal expansion coefficient
37.4
–
38.2
µstrain/°C
Thermal shock resistance
363
–
494
°C
Thermal distortion resistance
0.0134
–
0.014
MW/m
PA66 40% Long Glass Fiber Electrical properties
Electrical resistivity
2e17
–
5e18
µohm.cm
Electrical conductivity
3.45e-17
–
8.62e-16
%IACS
Dielectric constant (relative permittivity)
9.09
–
12.8
Dissipation factor (dielectric loss tangent)
0.127
–
0.334
Dielectric strength (dielectric breakdown)
31.8
–
54.2
MV/m
Comparative tracking index
525
–
575
V
PA66 40% Long Glass Fiber Magnetic properties
Magnetic type
Non-magnetic
PA66 40% Long Glass Fiber Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2470
–
2760
m/s
Mechanical loss coefficient (tan delta)
0.00815
–
0.00901
PA66 40% Long Glass Fiber Absorption & permeability