PA66 30-33% Glass Fiber Material Data Sheet

PA66 30-33% Glass Fiber (Polyamide 66) Material Data Sheet

PA66 30-33% Glass Fiber Overview

PA66 30-33% glass fiber is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 30-33% Glass Fiber). This PA66 30-33% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 30-33% Glass Fiber Designation

Polyamide (Nylon) (Type 66, 30-33% Glass Fiber)
TradenamesAkromid, Akulon, Alamid, Altech, Amilan, Anjacom, Anjamid, Ashlene, Badamid, Bergamid, Bestnyl, Celstran, Chemlon, Compamid, Domamid, Durethan, Eplamid, Germamid, Grilon, Kepamid, Kopa, LNP Thermocomp, Lumid, Next Prime, Nilamid, Niretan, Nivionplast, Novamid, Nylene, Nylfor, Nypol, Pentamid, Plustek, Polybest, Radilon, Ravamid, Razamid, Scanamid, Schulamid, Staramide, Taromid, Technyl, Tecomid, Terez, Ultramid, Vitamide, Wellamid, Zytel

PA66 30-33% Glass Fiber Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA66 30-33% Glass Fiber Composition detail

Polymer67–70%
Glass (fiber)30–33%

PA66 30-33% Glass Fiber Physical properties

Density1.35–1.38g/cm3

PA66 30-33% Glass Fiber Mechanical properties

Young’s modulus6.11–7.62GPa
Specific stiffness4.47–5.59MN.m/kg
Yield strength (elastic limit)138–140MPa
Tensile strength142–156MPa
Specific strength101–103kN.m/kg
Elongation4.73–5.5% strain
Elongation at yield4.25–4.93% strain
Compressive modulus6.55–7.23GPa
Compressive strength170–188MPa
Flexural modulus6.37–7.63GPa
Flexural strength (modulus of rupture)259–286MPa
Shear modulus2.46–2.59GPa
Shear strength84.8–93.8MPa
Bulk modulus7.2–7.95GPa
Poisson’s ratio0.34–0.36 
Shape factor5.3
Hardness – Vickers40–44HV
Hardness – Rockwell M84–92 
Hardness – Rockwell R111–123 
Hardness – Brinell117–147HB
Hardness – Shore D92–102 
Elastic stored energy (springs)1270–1580kJ/m3
Fatigue strength at 10^7 cycles56.5–62.5MPa

PA66 30-33% Glass Fiber Impact & fracture properties

Fracture toughness4.51–4.99MPa.m0.5
Toughness (G)2.85–3.81kJ/m2
Impact strength, notched 23 °C11.2–21.8kJ/m2
Impact strength, notched -30 °C6.93–15.1kJ/m2
Impact strength, unnotched 23 °C73.1–107kJ/m2
Impact strength, unnotched -30 °C53.3–80kJ/m2

PA66 30-33% Glass Fiber Thermal properties

Melting point260–265°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa252–279°C
Heat deflection temperature 1.8MPa227–254°C
Maximum service temperature90–130°C
Minimum service temperature-81–-71°C
Thermal conductivity0.4–0.49W/m.°C
Specific heat capacity1480–1530J/kg.°C
Thermal expansion coefficient27–97.2µstrain/°C
Thermal shock resistance209–757°C
Thermal distortion resistance0.00454–0.0165MW/m

PA66 30-33% Glass Fiber Electrical properties

Electrical resistivity1.97e19–4.92e20µohm.cm
Electrical conductivity3.5e-19–8.75e-18%IACS
Dielectric constant (relative permittivity)8.56–12.1 
Dissipation factor (dielectric loss tangent)0.136–0.358 
Dielectric strength (dielectric breakdown)27.8–47.3MV/m
Comparative tracking index450–600V

PA66 30-33% Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PA66 30-33% Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2110–2370m/s
Mechanical loss coefficient (tan delta)0.0095–0.0105 

PA66 30-33% Glass Fiber Absorption & permeability

Water absorption @ 24 hrs0.51–0.83%
Water absorption @ sat5–6.6%
Humidity absorption @ sat1.4–1.9%

PA66 30-33% Glass Fiber Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 0.6 %
Melt temperature220 – 304 °C
Mold temperature40 – 60 °C
Molding pressure range34.4 – 138 MPa

PA66 30-33% Glass Fiber Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySlow-burning