PA66 13-15% Glass Fiber (Polyamide 66) Material Data Sheet
PA66 13-15% Glass Fiber Overview
| PA66 13-15% glass fiber is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 13-15% Glass Fiber). This PA66 13-15% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment. |
PA66 13-15% Glass Fiber Designation
| Polyamide (Nylon) (Type 66, 13-15% Glass Fiber) | |
| Tradenames | Adell, Akromid, Akulon, Altech, Amilan, Anjamid, Ashlene, Bergamid, Bestnyl, Chemlon, Clariant, Durethan, Hylonselect, Kepamid, Kopa, Leona, LNP Thermocomp, Maxamid, Michimid, Next Prime, Nilamid, Nylfor, Nymax, Nypol, Pentamid, Plustek, Radilon, Scanamid, Schulamid, Slovamid, Staramide, Technyl, Ultramid, Vitamide, Wellamid, Zytel |
PA66 13-15% Glass Fiber Typical uses
| Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils. |
PA66 13-15% Glass Fiber Composition detail
| Polymer | 85 | – | 87 | % |
| Glass (fiber) | 13 | – | 15 | % |
PA66 13-15% Glass Fiber Physical properties
| Density | 1.22 | – | 1.24 | g/cm3 |
PA66 13-15% Glass Fiber Mechanical properties
| Young’s modulus | 3.46 | – | 4.31 | GPa |
| Specific stiffness | 2.81 | – | 3.51 | MN.m/kg |
| Yield strength (elastic limit) | 75.7 | – | 94.4 | MPa |
| Tensile strength | 72.7 | – | 88.8 | MPa |
| Specific strength | 61.5 | – | 76.8 | kN.m/kg |
| Elongation | 9.15 | – | 13.2 | % strain |
| Elongation at yield | 3.38 | – | 6.42 | % strain |
| Compressive modulus | 3.69 | – | 4.08 | GPa |
| Compressive strength | 92 | – | 102 | MPa |
| Flexural modulus | 3.19 | – | 3.82 | GPa |
| Flexural strength (modulus of rupture) | 90.1 | – | 110 | MPa |
| Shear modulus | 1.37 | – | 1.44 | GPa |
| Shear strength | 43.6 | – | 53.3 | MPa |
| Bulk modulus | 5.09 | – | 5.62 | GPa |
| Poisson’s ratio | 0.364 | – | 0.379 | |
| Shape factor | 5.05 | |||
| Hardness – Vickers | 24 | – | 27 | HV |
| Hardness – Rockwell M | 130 | – | 144 | |
| Hardness – Rockwell R | 130 | – | 144 | |
| Hardness – Brinell | 89 | – | 111 | HB |
| Hardness – Shore D | 85 | – | 89 | |
| Elastic stored energy (springs) | 734 | – | 1170 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 30.7 | – | 33.9 | MPa |
PA66 13-15% Glass Fiber Impact & fracture properties
| Fracture toughness | 4.02 | – | 4.45 | MPa.m0.5 |
| Toughness (G) | 4.01 | – | 5.36 | kJ/m2 |
| Impact strength, notched 23 °C | 6.27 | – | 12.2 | kJ/m2 |
| Impact strength, notched -30 °C | 4.56 | – | 9.92 | kJ/m2 |
| Impact strength, unnotched 23 °C | 55.6 | – | 81.7 | kJ/m2 |
| Impact strength, unnotched -30 °C | 34.7 | – | 52 | kJ/m2 |
PA66 13-15% Glass Fiber Thermal properties
| Melting point | 250 | – | 271 | °C |
| Glass temperature | 54 | – | 66 | °C |
| Heat deflection temperature 0.45MPa | 225 | – | 276 | °C |
| Heat deflection temperature 1.8MPa | 225 | – | 276 | °C |
| Maximum service temperature | 90 | – | 130 | °C |
| Minimum service temperature | -81 | – | -71 | °C |
| Thermal conductivity | 0.364 | – | 0.379 | W/m.°C |
| Specific heat capacity | 1510 | – | 1570 | J/kg.°C |
| Thermal expansion coefficient | 91.8 | – | 95.4 | µstrain/°C |
| Thermal shock resistance | 201 | – | 273 | °C |
| Thermal distortion resistance | 0.00386 | – | 0.00408 | MW/m |
PA66 13-15% Glass Fiber Electrical properties
| Electrical resistivity | 1.71e19 | – | 4.29e20 | µohm.cm |
| Electrical conductivity | 4.02e-19 | – | 1.01e-17 | %IACS |
| Dielectric constant (relative permittivity) | 7.61 | – | 10.7 | |
| Dissipation factor (dielectric loss tangent) | 0.0969 | – | 0.256 | |
| Dielectric strength (dielectric breakdown) | 33.8 | – | 57.6 | MV/m |
| Comparative tracking index | 450 | – | 550 | V |
PA66 13-15% Glass Fiber Magnetic properties
| Magnetic type | Non-magnetic |
PA66 13-15% Glass Fiber Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 1670 | – | 1880 | m/s |
| Mechanical loss coefficient (tan delta) | 0.0134 | – | 0.0148 | |
PA66 13-15% Glass Fiber Absorption & permeability
| Water absorption @ 24 hrs | 0.57 | – | 0.93 | % |
| Water absorption @ sat | 6.2 | – | 8.3 | % |
| Humidity absorption @ sat | 1.8 | – | 2.4 | % |
PA66 13-15% Glass Fiber Processing properties
| Polymer injection molding | Limited use |
| Polymer extrusion | Limited use |
| Polymer thermoforming | Limited use |
| Linear mold shrinkage | 0.364 – 0.44 % |
| Melt temperature | 226 – 302 °C |
| Mold temperature | 40 – 60 °C |
| Molding pressure range | 48.1 – 138 MPa |
PA66 13-15% Glass Fiber Durability
| Water (fresh) | Excellent |
| Water (salt) | Excellent |
| Weak acids | Unacceptable |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Acceptable |
| Organic solvents | Excellent |
| Oxidation at 500C | Unacceptable |
| UV radiation (sunlight) | Poor |
| Flammability | Slow-burning |