PA6 30-35% Glass Fiber Material Data Sheet

PA6 30-35% Glass Fiber (Polyamide 6) Material Data Sheet

PA6 30-35% Glass Fiber Overview

PA6 30-35% glass fiber is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 30-35% Glass Fiber). This PA6 30-35% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.

PA6 30-35% Glass Fiber Designation

Polyamide (Nylon) (Type 6, 30-35% Glass Fiber)
TradenamesAkromid, Akulon, Akulon Ultraflow, Alamid, Alcom, Altech, Amilan, Anjacom, Ashlene, Badamid, Bergamid, Bestnyl, Chemlon, Compamid, Deslon, Diaterm, Dilamid, Dinalon, Domamid, Durethan, Eplamid, Eplon, Germamid, Grilon, Grodnamid, Hifill, Isonyl, Kopa, Latamid, LNP Thermocomp, Lumid, Miramid, Next Industrial, Next Prime, Nilamid, Niretan, Nivionplast, Novamid, Novamide, Pentamid, Petlon Prime, Plustek, Polybest, Promyde, Radilon, Ravamid, Razamid, Scanamid, Schulamid, Silamid, Slovamid, Staramide, Tarnamid, Taromid, Technomid, Technyl, Technyl Star, Technylstar, Tecomid, Terez, Tufnyl, Ultramid, Vampamid, Vitamide, Wellamid, Witcom, Zytel

PA6 30-35% Glass Fiber Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 30-35% Glass Fiber Composition detail

Polymer65–70%
Glass (fiber)30–35%

PA6 30-35% Glass Fiber Physical properties

Density1.34–1.36g/cm3

PA6 30-35% Glass Fiber Mechanical properties

Young’s modulus5.34–6.66GPa
Specific stiffness3.95–4.93MN.m/kg
Yield strength (elastic limit)111–139MPa
Tensile strength108–132MPa
Specific strength82.2–103kN.m/kg
Elongation5.14–7.4% strain
Elongation at yield2.9–5.5% strain
Compressive modulus5.7–6.3GPa
Compressive strength137–151MPa
Flexural modulus4.87–5.84GPa
Flexural strength (modulus of rupture)147–179MPa
Shear modulus2.15–2.26GPa
Shear strength64.8–79.2MPa
Bulk modulus6.78–7.5GPa
Poisson’s ratio0.34–0.36 
Shape factor5.19
Hardness – Vickers36–39HV
Hardness – Rockwell M158–175 
Hardness – Rockwell R158–175 
Hardness – Brinell96–120HB
Hardness – Shore D92–96 
Elastic stored energy (springs)1020–1640kJ/m3
Fatigue strength at 10^7 cycles45.6–50.4MPa

PA6 30-35% Glass Fiber Impact & fracture properties

Fracture toughness4.39–4.85MPa.m0.5
Toughness (G)3.09–4.12kJ/m2
Impact strength, notched 23 °C14–27.2kJ/m2
Impact strength, notched -30 °C6.9–15kJ/m2
Impact strength, unnotched 23 °C77.6–114kJ/m2
Impact strength, unnotched -30 °C54.1–81.2kJ/m2

PA6 30-35% Glass Fiber Thermal properties

Melting point210–220°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa216–221°C
Heat deflection temperature 1.8MPa200–216°C
Maximum service temperature90–130°C
Minimum service temperature-64–-54°C
Thermal conductivity0.243–0.477W/m.°C
Specific heat capacity1390–1440J/kg.°C
Thermal expansion coefficient28.8–144µstrain/°C
Thermal shock resistance144–727°C
Thermal distortion resistance0.0023–0.0122MW/m

PA6 30-35% Glass Fiber Electrical properties

Electrical resistivity2.53e19–6.32e20µohm.cm
Electrical conductivity2.73e-19–6.81e-18%IACS
Dielectric constant (relative permittivity)10.1–14.2 
Dissipation factor (dielectric loss tangent)0.117–0.309 
Dielectric strength (dielectric breakdown)25.1–42.7MV/m
Comparative tracking index450–600V

PA6 30-35% Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PA6 30-35% Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1990–2220m/s
Mechanical loss coefficient (tan delta)0.0109–0.012 

PA6 30-35% Glass Fiber Absorption & permeability

Water absorption @ 24 hrs1.2–2%
Water absorption @ sat5.4–7.2%
Humidity absorption @ sat1.7–2.3%

PA6 30-35% Glass Fiber Processing properties

Polymer injection moldingExcellent
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.1 – 0.2 %
Melt temperature198 – 288 °C
Mold temperature50 – 60 °C
Molding pressure range13.8 – 138 MPa

PA6 30-35% Glass Fiber Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning