PA6 40% Long Glass Fiber (Polyamide 6) Material Data Sheet
PA6 40% Long Glass Fiber Overview
PA6 40% long glass fiber is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 40% Long Glass Fiber). This PA6 40% long glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.
PA6 40% Long Glass Fiber Designation
Polyamide (Nylon) (Type 6, 40% Long Glass Fiber)
Tradenames
Celstran, Complet, Sepaz, Stranox
PA6 40% Long Glass Fiber Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA6 40% Long Glass Fiber Composition detail
Polymer
60
%
Glass (fiber)
40
%
PA6 40% Long Glass Fiber Physical properties
Density
1.44
–
1.47
g/cm3
PA6 40% Long Glass Fiber Mechanical properties
Young’s modulus
8.28
–
10.3
GPa
Specific stiffness
5.69
–
7.08
MN.m/kg
Yield strength (elastic limit)
130
–
162
MPa
Tensile strength
131
–
161
MPa
Specific strength
89.3
–
111
kN.m/kg
Elongation
1.8
–
2.6
% strain
Elongation at yield
1.52
–
2.88
% strain
Compressive modulus
8.84
–
9.77
GPa
Compressive strength
166
–
184
MPa
Flexural modulus
7.83
–
9.37
GPa
Flexural strength (modulus of rupture)
212
–
259
MPa
Shear modulus
3.33
–
3.5
GPa
Shear strength
78.8
–
96.4
MPa
Bulk modulus
10.5
–
11.6
GPa
Poisson’s ratio
0.34
–
0.36
Shape factor
6.11
Hardness – Vickers
42
–
46
HV
Hardness – Rockwell M
174
–
192
Hardness – Rockwell R
174
–
192
Hardness – Shore D
96
–
100
Elastic stored energy (springs)
905
–
1440
kJ/m3
Fatigue strength at 10^7 cycles
55.5
–
61.3
MPa
PA6 40% Long Glass Fiber Impact & fracture properties
Fracture toughness
4.8
–
5.3
MPa.m0.5
Toughness (G)
2.39
–
3.18
kJ/m2
Impact strength, notched 23 °C
21.8
–
42.2
kJ/m2
Impact strength, notched -30 °C
2.66
–
5.77
kJ/m2
Impact strength, unnotched 23 °C
51.6
–
75.9
kJ/m2
Impact strength, unnotched -30 °C
34.9
–
52.3
kJ/m2
PA6 40% Long Glass Fiber Thermal properties
Melting point
210
–
271
°C
Glass temperature
44
–
56
°C
Heat deflection temperature 0.45MPa
209
–
258
°C
Heat deflection temperature 1.8MPa
184
–
231
°C
Maximum service temperature
90
–
130
°C
Minimum service temperature
-64
–
-54
°C
Thermal conductivity
0.514
–
0.534
W/m.°C
Specific heat capacity
1340
–
1400
J/kg.°C
Thermal expansion coefficient
36.5
–
37.3
µstrain/°C
Thermal shock resistance
366
–
496
°C
Thermal distortion resistance
0.0139
–
0.0145
MW/m
PA6 40% Long Glass Fiber Electrical properties
Electrical resistivity
1.2e19
–
3e20
µohm.cm
Electrical conductivity
5.75e-19
–
1.44e-17
%IACS
Dielectric constant (relative permittivity)
9.63
–
13.6
Dissipation factor (dielectric loss tangent)
0.138
–
0.365
Dielectric strength (dielectric breakdown)
28.1
–
47.9
MV/m
Comparative tracking index
425
–
475
V
PA6 40% Long Glass Fiber Magnetic properties
Magnetic type
Non-magnetic
PA6 40% Long Glass Fiber Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2380
–
2670
m/s
Mechanical loss coefficient (tan delta)
0.00857
–
0.00947
PA6 40% Long Glass Fiber Absorption & permeability