PA6 30% Long Glass Fiber (Polyamide 6) Material Data Sheet
PA6 30% Long Glass Fiber Overview
PA6 30% long glass fiber is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 30% Long Glass Fiber). This PA6 30% long glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.
PA6 30% Long Glass Fiber Designation
Polyamide (Nylon) (Type 6, 30% Long Glass Fiber)
Tradenames
Celstran, Complet, Sepaz, Stranox
PA6 30% Long Glass Fiber Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA6 30% Long Glass Fiber Composition detail
Polymer
70
%
Glass (fiber)
30
%
PA6 30% Long Glass Fiber Physical properties
Density
1.34
–
1.37
g/cm3
PA6 30% Long Glass Fiber Mechanical properties
Young’s modulus
6.5
–
8.1
GPa
Specific stiffness
4.8
–
5.98
MN.m/kg
Yield strength (elastic limit)
111
–
139
MPa
Tensile strength
113
–
138
MPa
Specific strength
81.9
–
103
kN.m/kg
Elongation
2.81
–
4.05
% strain
Elongation at yield
2.37
–
4.5
% strain
Compressive modulus
6.94
–
7.67
GPa
Compressive strength
143
–
158
MPa
Flexural modulus
5.82
–
6.98
GPa
Flexural strength (modulus of rupture)
176
–
215
MPa
Shear modulus
2.62
–
2.75
GPa
Shear strength
67.5
–
82.5
MPa
Bulk modulus
8.26
–
9.13
GPa
Poisson’s ratio
0.34
–
0.36
Shape factor
5.8
Hardness – Vickers
36
–
39
HV
Hardness – Rockwell M
161
–
178
Hardness – Rockwell R
161
–
178
Hardness – Shore D
93
–
97
Elastic stored energy (springs)
840
–
1340
kJ/m3
Fatigue strength at 10^7 cycles
47.5
–
52.5
MPa
PA6 30% Long Glass Fiber Impact & fracture properties
Fracture toughness
4.57
–
5.05
MPa.m0.5
Toughness (G)
2.75
–
3.67
kJ/m2
Impact strength, notched 23 °C
23.8
–
46.2
kJ/m2
Impact strength, notched -30 °C
6.72
–
14.6
kJ/m2
Impact strength, unnotched 23 °C
46.8
–
68.8
kJ/m2
Impact strength, unnotched -30 °C
37.3
–
56
kJ/m2
PA6 30% Long Glass Fiber Thermal properties
Melting point
210
–
220
°C
Glass temperature
44
–
56
°C
Heat deflection temperature 0.45MPa
195
–
220
°C
Heat deflection temperature 1.8MPa
192
–
240
°C
Maximum service temperature
90
–
130
°C
Minimum service temperature
-64
–
-54
°C
Thermal conductivity
0.445
–
0.463
W/m.°C
Specific heat capacity
1350
–
1450
J/kg.°C
Thermal expansion coefficient
38.9
–
40.3
µstrain/°C
Thermal shock resistance
370
–
505
°C
Thermal distortion resistance
0.0112
–
0.0118
MW/m
PA6 30% Long Glass Fiber Electrical properties
Electrical resistivity
2.53e19
–
6.32e20
µohm.cm
Electrical conductivity
2.73e-19
–
6.81e-18
%IACS
Dielectric constant (relative permittivity)
10.1
–
14.2
Dissipation factor (dielectric loss tangent)
0.117
–
0.309
Dielectric strength (dielectric breakdown)
25.1
–
42.7
MV/m
Comparative tracking index
500
–
550
V
PA6 30% Long Glass Fiber Magnetic properties
Magnetic type
Non-magnetic
PA6 30% Long Glass Fiber Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
2190
–
2450
m/s
Mechanical loss coefficient (tan delta)
0.00994
–
0.011
PA6 30% Long Glass Fiber Absorption & permeability