PA6 50% Glass Fiber Material Data Sheet

PA6 50% Glass Fiber (Polyamide 6) Material Data Sheet

PA6 50% Glass Fiber Overview

PA6 50% glass fiber is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 50% Glass Fiber). This PA6 50% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.

PA6 50% Glass Fiber Designation

Polyamide (Nylon) (Type 6, 50% Glass Fiber)
TradenamesAkromid, Akulon, Akulon Ultraflow, Anjacom, Badamid, Bergamid, Bestnyl, Celstran, Chemlon, Domamid, Durethan, Grilon, Hifill, Niretan, Novamid, Nylaforce, Pentamid, Petlon R-Prime, Plustek, Polybest, Radilon, Scanamid, Schulamid, Slovamid, Staramide, Tarnamid, Technyl, Technyl Star, Technylstar, Terez, Ultramid, Vitamide, Wellamid

PA6 50% Glass Fiber Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 50% Glass Fiber Composition detail

Polymer50  %
Glass (fiber)50  %

PA6 50% Glass Fiber Physical properties

Density1.56–1.6g/cm3

PA6 50% Glass Fiber Mechanical properties

Young’s modulus9.5–11.8GPa
Specific stiffness6.01–7.47MN.m/kg
Yield strength (elastic limit)137–171MPa
Tensile strength138–169MPa
Specific strength86.7–108kN.m/kg
Elongation3.47–4.99% strain
Elongation at yield2.92–5.54% strain
Compressive modulus10.1–11.2GPa
Compressive strength175–194MPa
Flexural modulus8.71–10.4GPa
Flexural strength (modulus of rupture)201–246MPa
Shear modulus3.83–4.02GPa
Shear strength83.1–102MPa
Bulk modulus12.1–13.3GPa
Poisson’s ratio0.34–0.36 
Shape factor6.4
Hardness – Vickers44–49HV
Hardness – Rockwell M178–197 
Hardness – Rockwell R178–197 
Hardness – Brinell97–121HB
Hardness – Shore D97–101 
Elastic stored energy (springs)877–1390kJ/m3
Fatigue strength at 10^7 cycles58.5–64.6MPa

PA6 50% Glass Fiber Impact & fracture properties

Fracture toughness4.94–5.45MPa.m0.5
Toughness (G)2.21–2.93kJ/m2
Impact strength, notched 23 °C17.3–33.5kJ/m2
Impact strength, notched -30 °C8.82–19.2kJ/m2
Impact strength, unnotched 23 °C84.6–124kJ/m2
Impact strength, unnotched -30 °C70.8–106kJ/m2

PA6 50% Glass Fiber Thermal properties

Melting point210–230°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa197–245°C
Heat deflection temperature 1.8MPa192–239°C
Maximum service temperature90–130°C
Minimum service temperature-64–-54°C
Thermal conductivity0.521–0.542W/m.°C
Specific heat capacity1280–1330J/kg.°C
Thermal expansion coefficient52.9–55.1µstrain/°C
Thermal shock resistance230–312°C
Thermal distortion resistance0.00957–0.0101MW/m

PA6 50% Glass Fiber Electrical properties

Electrical resistivity1.32e19–3.31e20µohm.cm
Electrical conductivity5.21e-19–1.31e-17%IACS
Dielectric constant (relative permittivity)9.2–13 
Dissipation factor (dielectric loss tangent)0.116–0.305 
Dielectric strength (dielectric breakdown)28.6–48.8MV/m
Comparative tracking index450–600V

PA6 50% Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PA6 50% Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2450–2740m/s
Mechanical loss coefficient (tan delta)0.00812–0.00898 

PA6 50% Glass Fiber Absorption & permeability

Water absorption @ 24 hrs0.93–1.5%
Water absorption @ sat4.1–5.4%
Humidity absorption @ sat1.2–1.7%

PA6 50% Glass Fiber Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.091 – 0.11 %
Melt temperature226 – 302 °C
Mold temperature50 – 60 °C
Molding pressure range68.8 – 138 MPa

PA6 50% Glass Fiber Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning