Home » PA (Polyamide / Nylon) » PA6 (Polyamide 6 / Nylon 6) » PA6 Glass Filled Grades » PA6 30% Glass Fiber Impact Modified Material Data Sheet
PA6 30% Glass Fiber Impact Modified (Polyamide 6) Material Data Sheet
PA6 30% Glass Fiber Impact Modified Overview
PA6 30% glass fiber impact modified is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 30% Glass Fiber, Impact Modified). This PA6 30% glass fiber impact modified material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.
PA6 30% Glass Fiber Impact Modified Designation
Polyamide (Nylon) (Type 6, 30% Glass Fiber, Impact Modified) Tradenames Akulon, Altech, Chemlon, Domamid, Durethan, Grilon, Mapex, Pentamid, Schulamid, Taromid, Tecomid, Terez, Ultramid, Vitamide, Zytel
PA6 30% Glass Fiber Impact Modified Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA6 30% Glass Fiber Impact Modified Composition detail
Polymer 55 – 67 % Impact modifier 3 – 15 % Glass (fiber) 30 %
PA6 30% Glass Fiber Impact Modified Physical properties
PA6 30% Glass Fiber Impact Modified Mechanical properties
Young’s modulus 4.74 – 5.91 GPa Specific stiffness 3.65 – 4.55 MN.m/kg Yield strength (elastic limit) 88.7 – 111 MPa Tensile strength 89.6 – 110 MPa Specific strength 68.2 – 85.4 kN.m/kg Elongation 6.35 – 9.14 % strain Elongation at yield 5.34 – 10.1 % strain Compressive modulus 5.06 – 5.59 GPa Compressive strength 114 – 126 MPa Flexural modulus 4.31 – 5.16 GPa Flexural strength (modulus of rupture) 131 – 160 MPa Shear modulus 1.91 – 2.01 GPa Shear strength 53.8 – 65.7 MPa Bulk modulus 6.02 – 6.65 GPa Poisson’s ratio 0.34 – 0.36 Shape factor 5.51 Hardness – Vickers 28 – 31 HV Hardness – Rockwell M 145 – 160 Hardness – Rockwell R 145 – 160 Hardness – Brinell 71 – 89 HB Hardness – Shore D 89 – 93 Elastic stored energy (springs) 736 – 1180 kJ/m3 Fatigue strength at 10^7 cycles 37.9 – 41.8 MPa
PA6 30% Glass Fiber Impact Modified Impact & fracture properties
Fracture toughness 4.29 – 4.74 MPa.m0.5 Toughness (G) 3.33 – 4.44 kJ/m2 Impact strength, notched 23 °C 22.1 – 42.8 kJ/m2 Impact strength, notched -30 °C 9.61 – 20.9 kJ/m2 Impact strength, unnotched 23 °C 82.7 – 121 kJ/m2 Impact strength, unnotched -30 °C 68 – 102 kJ/m2
PA6 30% Glass Fiber Impact Modified Thermal properties
Melting point 210 – 220 °C Glass temperature 44 – 56 °C Heat deflection temperature 0.45MPa 197 – 220 °C Heat deflection temperature 1.8MPa 187 – 234 °C Maximum service temperature 57 – 77 °C Minimum service temperature -64 – -54 °C Thermal conductivity 0.426 – 0.443 W/m.°C Specific heat capacity 1430 – 1490 J/kg.°C Thermal expansion coefficient 36 – 45 µstrain/°C Thermal shock resistance 387 – 561 °C Thermal distortion resistance 0.00964 – 0.0121 MW/m
PA6 30% Glass Fiber Impact Modified Electrical properties
Electrical resistivity 1.16e19 – 2.89e20 µohm.cm Electrical conductivity 5.97e-19 – 1.49e-17 %IACS Dielectric constant (relative permittivity) 10.1 – 14.2 Dissipation factor (dielectric loss tangent) 0.133 – 0.351 Dielectric strength (dielectric breakdown) 24.1 – 41 MV/m Comparative tracking index 500 – 600 V
PA6 30% Glass Fiber Impact Modified Magnetic properties
Magnetic type Non-magnetic
PA6 30% Glass Fiber Impact Modified Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 1910 – 2140 m/s Mechanical loss coefficient (tan delta) 0.0116 – 0.0128
PA6 30% Glass Fiber Impact Modified Absorption & permeability
Water absorption @ 24 hrs 1.2 – 2 % Water absorption @ sat 5.4 – 7.1 % Humidity absorption @ sat 1.6 – 2.1 %
PA6 30% Glass Fiber Impact Modified Processing properties
Polymer injection molding Excellent Polymer extrusion Limited use Polymer thermoforming Limited use Linear mold shrinkage 0.3 – 0.5 % Melt temperature 205 – 288 °C Mold temperature 50 – 60 °C Molding pressure range 20.6 – 138 MPa
PA6 30% Glass Fiber Impact Modified Durability
Water (fresh) Excellent Water (salt) Acceptable Weak acids Unacceptable Strong acids Unacceptable Weak alkalis Limited use Strong alkalis Limited use Organic solvents Acceptable Oxidation at 500C Unacceptable UV radiation (sunlight) Fair Flammability Slow-burning