Home » PA (Polyamide / Nylon) » PA6 (Polyamide 6 / Nylon 6) » PA6 Glass Filled Grades » PA6 30% Glass Fiber Flame Retarded Material Data Sheet
PA6 30% Glass Fiber Flame Retarded (Polyamide 6) Material Data Sheet
PA6 30% Glass Fiber Flame Retarded Overview
PA6 30% glass fiber flame retarded is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 30% Glass Fiber, Flame Retarded). This PA6 30% glass fiber flame retarded material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.
PA6 30% Glass Fiber Flame Retarded Designation
Polyamide (Nylon) (Type 6, 30% Glass Fiber, Flame Retarded) Tradenames Abel, Akulon, Akulon Ultraflow, Cheng, Dinalon, Domamid, Durethan, Eplamid, Frblend, Frianyl, Novamid, Nylfor, Radiflam, Schulamid, Slovamid, Tarnamid
PA6 30% Glass Fiber Flame Retarded Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA6 30% Glass Fiber Flame Retarded Composition detail
Polymer 55 – 65 % Flame retardant 5 – 15 % Glass (fiber) 30 %
PA6 30% Glass Fiber Flame Retarded Physical properties
PA6 30% Glass Fiber Flame Retarded Mechanical properties
Young’s modulus 6.8 – 8.48 GPa Specific stiffness 4.4 – 5.49 MN.m/kg Yield strength (elastic limit) 71.2 – 88.8 MPa Tensile strength 83.1 – 102 MPa Specific strength 46.1 – 57.5 kN.m/kg Elongation 2.87 – 4.13 % strain Elongation at yield 2.42 – 4.59 % strain Compressive modulus 7.26 – 8.03 GPa Compressive strength 105 – 116 MPa Flexural modulus 4.61 – 5.52 GPa Flexural strength (modulus of rupture) 104 – 127 MPa Shear modulus 2.74 – 2.88 GPa Shear strength 49.9 – 61 MPa Bulk modulus 8.64 – 9.55 GPa Poisson’s ratio 0.34 – 0.36 Shape factor 7.9 Hardness – Vickers 23 – 25 HV Hardness – Rockwell M 139 – 154 Hardness – Rockwell R 139 – 154 Hardness – Shore D 88 – 91 Elastic stored energy (springs) 330 – 525 kJ/m3 Fatigue strength at 10^7 cycles 35.1 – 38.8 MPa
PA6 30% Glass Fiber Flame Retarded Impact & fracture properties
Fracture toughness 4.61 – 5.1 MPa.m0.5 Toughness (G) 2.68 – 3.58 kJ/m2 Impact strength, notched 23 °C 8.43 – 16.4 kJ/m2 Impact strength, notched -30 °C 6.72 – 14.6 kJ/m2 Impact strength, unnotched 23 °C 46.8 – 68.8 kJ/m2 Impact strength, unnotched -30 °C 37.3 – 56 kJ/m2
PA6 30% Glass Fiber Flame Retarded Thermal properties
Melting point 210 – 220 °C Glass temperature 44 – 56 °C Heat deflection temperature 0.45MPa 192 – 220 °C Heat deflection temperature 1.8MPa 193 – 204 °C Maximum service temperature 90 – 130 °C Minimum service temperature -64 – -54 °C Thermal conductivity 0.494 – 0.514 W/m.°C Specific heat capacity 1220 – 1270 J/kg.°C Thermal expansion coefficient 39.2 – 40 µstrain/°C Thermal shock resistance 227 – 308 °C Thermal distortion resistance 0.0125 – 0.013 MW/m
PA6 30% Glass Fiber Flame Retarded Electrical properties
Electrical resistivity 3.41e19 – 8.52e20 µohm.cm Electrical conductivity 2.02e-19 – 5.06e-18 %IACS Dielectric constant (relative permittivity) 7.47 – 10.5 Dissipation factor (dielectric loss tangent) 0.118 – 0.312 Dielectric strength (dielectric breakdown) 20 – 34 MV/m Comparative tracking index 250 – 600 V
PA6 30% Glass Fiber Flame Retarded Magnetic properties
Magnetic type Non-magnetic
PA6 30% Glass Fiber Flame Retarded Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 2090 – 2350 m/s Mechanical loss coefficient (tan delta) 0.0112 – 0.0123
PA6 30% Glass Fiber Flame Retarded Absorption & permeability
Water absorption @ 24 hrs 0.86 – 1.4 % Water absorption @ sat 3.8 – 5 % Humidity absorption @ sat 1.2 – 1.6 %
PA6 30% Glass Fiber Flame Retarded Processing properties
Polymer injection molding Excellent Polymer extrusion Limited use Polymer thermoforming Limited use Linear mold shrinkage 0.091 – 0.11 % Melt temperature 217 – 293 °C Mold temperature 50 – 60 °C Molding pressure range 82.5 – 172 MPa
PA6 30% Glass Fiber Flame Retarded Durability
Water (fresh) Excellent Water (salt) Acceptable Weak acids Unacceptable Strong acids Unacceptable Weak alkalis Limited use Strong alkalis Limited use Organic solvents Acceptable Oxidation at 500C Unacceptable UV radiation (sunlight) Fair Flammability Self-extinguishing