Home » PA (Polyamide / Nylon) » PA6 (Polyamide 6 / Nylon 6) » PA6 Glass Filled Grades » PA6 25% Glass Fiber Material Data Sheet
PA6 25% Glass Fiber (Polyamide 6) Material Data Sheet
PA6 25% Glass Fiber Overview
PA6 25% glass fiber is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 25% Glass Fiber). This PA6 25% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.
PA6 25% Glass Fiber Designation
Polyamide (Nylon) (Type 6, 25% Glass Fiber) Tradenames Akromid, Akulon, Akulon Ultraflow, Alamid, Altech, Anjacom, Ashlene, Bergamid, Bestnyl, Chemlon, Dinalon, Durethan, Grilon, Kepamid, Pentamid, Petlon Prime, Radilon, Scanamid, Schulamid, Slovamid, Staramide, Tarnamid, Taromid, Ultramid, Vitamide, Wellamid
PA6 25% Glass Fiber Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA6 25% Glass Fiber Composition detail
Polymer 75 % Glass (fiber) 25 %
PA6 25% Glass Fiber Physical properties
PA6 25% Glass Fiber Mechanical properties
Young’s modulus 3.8 – 4.75 GPa Specific stiffness 3.02 – 3.77 MN.m/kg Yield strength (elastic limit) 80.1 – 99.9 MPa Tensile strength 77.7 – 94.9 MPa Specific strength 63.6 – 79.3 kN.m/kg Elongation 5.02 – 7.23 % strain Elongation at yield 3.17 – 6.03 % strain Compressive modulus 4.06 – 4.49 GPa Compressive strength 98.4 – 109 MPa Flexural modulus 3.85 – 4.61 GPa Flexural strength (modulus of rupture) 128 – 157 MPa Shear modulus 1.53 – 1.61 GPa Shear strength 46.6 – 56.9 MPa Bulk modulus 4.83 – 5.34 GPa Poisson’s ratio 0.34 – 0.36 Shape factor 5.2 Hardness – Vickers 26 – 28 HV Hardness – Rockwell M 134 – 149 Hardness – Rockwell R 134 – 149 Hardness – Brinell 96 – 119 HB Hardness – Shore D 87 – 90 Elastic stored energy (springs) 746 – 1190 kJ/m3 Fatigue strength at 10^7 cycles 32.8 – 36.2 MPa
PA6 25% Glass Fiber Impact & fracture properties
Fracture toughness 4.1 – 4.53 MPa.m0.5 Toughness (G) 3.78 – 5.05 kJ/m2 Impact strength, notched 23 °C 12.8 – 24.8 kJ/m2 Impact strength, notched -30 °C 3.59 – 7.81 kJ/m2 Impact strength, unnotched 23 °C 66.4 – 97.6 kJ/m2 Impact strength, unnotched -30 °C 33.6 – 50.4 kJ/m2
PA6 25% Glass Fiber Thermal properties
Melting point 210 – 230 °C Glass temperature 44 – 56 °C Heat deflection temperature 0.45MPa 197 – 230 °C Heat deflection temperature 1.8MPa 187 – 234 °C Maximum service temperature 90 – 130 °C Minimum service temperature -64 – -54 °C Thermal conductivity 0.417 – 0.433 W/m.°C Specific heat capacity 1440 – 1490 J/kg.°C Thermal expansion coefficient 70.6 – 73.4 µstrain/°C Thermal shock resistance 251 – 341 °C Thermal distortion resistance 0.00574 – 0.00607 MW/m
PA6 25% Glass Fiber Electrical properties
Electrical resistivity 2.51e19 – 6.28e20 µohm.cm Electrical conductivity 2.75e-19 – 6.87e-18 %IACS Dielectric constant (relative permittivity) 7.75 – 10.9 Dissipation factor (dielectric loss tangent) 0.121 – 0.319 Dielectric strength (dielectric breakdown) 34 – 58 MV/m Comparative tracking index 500 – 550 V
PA6 25% Glass Fiber Magnetic properties
Magnetic type Non-magnetic
PA6 25% Glass Fiber Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 1730 – 1940 m/s Mechanical loss coefficient (tan delta) 0.0122 – 0.0135
PA6 25% Glass Fiber Absorption & permeability
Water absorption @ 24 hrs 1.6 – 2.6 % Water absorption @ sat 6.9 – 9.1 % Humidity absorption @ sat 2 – 2.8 %
PA6 25% Glass Fiber Processing properties
Polymer injection molding Excellent Polymer extrusion Limited use Polymer thermoforming Limited use Linear mold shrinkage 0.182 – 0.22 % Melt temperature 220 – 291 °C Mold temperature 50 – 60 °C Molding pressure range 20.6 – 138 MPa
PA6 25% Glass Fiber Durability
Water (fresh) Excellent Water (salt) Acceptable Weak acids Unacceptable Strong acids Unacceptable Weak alkalis Limited use Strong alkalis Limited use Organic solvents Acceptable Oxidation at 500C Unacceptable UV radiation (sunlight) Fair Flammability Slow-burning
Modulus Metal Services