PA6 15% Glass Fiber Material Data Sheet

PA6 15% Glass Fiber (Polyamide 6) Material Data Sheet

PA6 15% Glass Fiber Overview

PA6 15% glass fiber is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 15% Glass Fiber). This PA6 15% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.

PA6 15% Glass Fiber Designation

Polyamide (Nylon) (Type 6, 15% Glass Fiber)
TradenamesAdell, Akromid, Akulon, Altech, Amilan, Anjacom, Anjamid, Bergamid, Bestnyl, Chemlon, Domamid, Durethan, Grilon, Hifill, Hylonselect, Kopa, Lumid, Novamid, Nycal, Nylene, Pentamid, Petlon Prime, Plustek, Polybest, Promyde, Ravamid, Scanamid, Schulamid, Staramide, Tarnamid, Technyl, Tecomid, Terez, Tufnyl, Ultramid, Vitamide, Wellamid, Zytel

PA6 15% Glass Fiber Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 15% Glass Fiber Composition detail

Polymer85  %
Glass (fiber)15  %

PA6 15% Glass Fiber Physical properties

Density1.22–1.24g/cm3

PA6 15% Glass Fiber Mechanical properties

Young’s modulus3.13–3.91GPa
Specific stiffness2.54–3.18MN.m/kg
Yield strength (elastic limit)68.5–85.5MPa
Tensile strength63.9–78.1MPa
Specific strength55.7–69.5kN.m/kg
Elongation8.44–12.1% strain
Elongation at yield2.83–5.37% strain
Compressive modulus3.35–3.7GPa
Compressive strength81–89.5MPa
Flexural modulus2.64–3.16GPa
Flexural strength (modulus of rupture)99–121MPa
Shear modulus1.26–1.33GPa
Shear strength38.4–46.9MPa
Bulk modulus3.98–4.4GPa
Poisson’s ratio0.34–0.36 
Shape factor5.1
Hardness – Vickers22–24HV
Hardness – Rockwell M121–134 
Hardness – Rockwell R121–134 
Hardness – Brinell71–89HB
Hardness – Shore D83–87 
Elastic stored energy (springs)663–1060kJ/m3
Fatigue strength at 10^7 cycles27–29.8MPa

PA6 15% Glass Fiber Impact & fracture properties

Fracture toughness3.94–4.36MPa.m0.5
Toughness (G)4.24–5.68kJ/m2
Impact strength, notched 23 °C9.66–18.8kJ/m2
Impact strength, notched -30 °C5.15–11.2kJ/m2
Impact strength, unnotched 23 °C83.5–123kJ/m2
Impact strength, unnotched -30 °C30.7–46.1kJ/m2

PA6 15% Glass Fiber Thermal properties

Melting point210–230°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa192–230°C
Heat deflection temperature 1.8MPa168–213°C
Maximum service temperature90–130°C
Minimum service temperature-64–-54°C
Thermal conductivity0.353–0.367W/m.°C
Specific heat capacity1510–1570J/kg.°C
Thermal expansion coefficient91.8–95.4µstrain/°C
Thermal shock resistance200–273°C
Thermal distortion resistance0.00374–0.00396MW/m

PA6 15% Glass Fiber Electrical properties

Electrical resistivity2.75e19–6.87e20µohm.cm
Electrical conductivity2.51e-19–6.27e-18%IACS
Dielectric constant (relative permittivity)8.36–11.8 
Dissipation factor (dielectric loss tangent)0.0776–0.204 
Dielectric strength (dielectric breakdown)25–42.5MV/m
Comparative tracking index400–600V

PA6 15% Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PA6 15% Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1590–1790m/s
Mechanical loss coefficient (tan delta)0.0148–0.0163 

PA6 15% Glass Fiber Absorption & permeability

Water absorption @ 24 hrs1.6–2.6%
Water absorption @ sat6.9–9.2%
Humidity absorption @ sat2–2.7%

PA6 15% Glass Fiber Processing properties

Polymer injection moldingExcellent
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 0.3 %
Melt temperature220 – 291 °C
Mold temperature50 – 60 °C
Molding pressure range20.6 – 138 MPa

PA6 15% Glass Fiber Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning