PEEK (Polyetheretherketone)

PEEK (Polyetheretherketone)

PEEK Overview

PEEK (polyetheretherketone) is a high-performance semi-crystalline thermoplastic. Commercial PEEK types differ mainly in their melting temperature. A higher melting point gives a higher heat distortion temperature but also requires a higher processing temperature. PEEK has replaced aluminum and other metals in many applications, especially in aviation.

PEEK Strengths

PEEK resists most chemicals except concentrated acids, withstands hydrolysis better than PEIs, and has excellent UV and radiation resistance. Its maximum service temperature is very high, about 260 °C (500 °F), and its oxidative stability at high temperature is matched only by PPS and LCP. It is inherently flame retardant, with very low smoke and toxic gas emission. Toughness, wear resistance, fatigue and dynamic fatigue resistance and tracking resistance are excellent, it resists cutting as a wire covering, and its strength-to-weight ratio is higher than that of many metals.

PEEK Limitations

Concentrated acids attack PEEK. It is expensive, difficult to process and available from a limited number of suppliers. It is notch sensitive and can stress crack in concentrated sodium hydroxide, glycerol, sodium carbonate solution, ethyl acetate and aniline, with moderate stress cracking risk in ethanol, cyclohexanone and chloromethane.

PEEK Designation

PEEK belongs to the polyaryl ether ketones (polyether ketones). Tradenames include Ketron PEEK, Thermocomp, Victrex and PEEK-Optima.

Typical Uses of PEEK

Aerospace parts, medical implants, wire insulation, injection-molded engineering components, flexible PCB film, prepreg resins, piping and parts for radiation environments. Filled grades are used for lightweight structural parts in aerospace, ground transport and sporting goods, as well as springs and pressure vessels.

PEEK Compositional Summary

(-C6H4-O-C6H4-O-C6H4-(C=O)-)n
Material familyPlastic (thermoplastic, semi-crystalline)
Base materialPEEK (Polyetheretherketone)
CAS number31694-16-3

Effect of Composition on PEEK

Adding 10–20% PTFE can bring the friction coefficient down close to that of PTFE, and static and dynamic friction values move closer together, which reduces stick-slip. PEEK is fully miscible with polyether ketones whose keto content is within 25% of its own (8–58%), so it blends with PEK but not with PEKK. It is also fully miscible with PEI, and these blends have higher impact resistance than either component.

PEEK Notes

The natural colour is beige to brown. Ultra-pure grades are used for medical implants.

PEEK Processing Properties

First Commercial Production

1983

Available Forms

Pellets and powder, plus rods and plates for machining.

Forming

PEEK can be compression molded, extruded and vacuum formed, while injection molding is difficult. It needs very high melt temperatures (370 °C (700 °F) or above) and pre-drying is essential because of the high mold temperatures. Fine powder can coat metal parts up to about 2 mm thick by vortex sintering.

Machining

The material machines very easily. Carbide or diamond-tipped tools with water cooling are recommended, and the parts should be annealed before machining.

Joining

Solvent bonding is difficult, but a wide range of adhesives works well, and surface treatment such as laser treatment greatly improves bond strength. All welding methods except radio-frequency welding are suitable, although hot gas welding is difficult and the high melting point means welding needs a lot of energy. Laser welding works, the material can be welded to PEI, and welds to aluminum have had some success. Films can be heat sealed at high temperatures.

Surface Treatment

PEEK can be painted.

PEEK Grades

Unfilled PEEK

PEEK (unfilled)

Glass Filled PEEK

PEEK (10% glass fiber)

PEEK (15% glass fiber)

PEEK (30% glass fiber)

Carbon Filled PEEK

PEEK (30% carbon fiber)

PEEK (30% carbon fiber, lubricated)

PEEK (40% carbon fiber)

Modified PEEK Blends, Unfilled

PEEK-modified (unfilled)

Modified PEEK Blends, Glass Filled

PEEK-modified (30% glass fiber)

PEEK-modified (40% glass fiber)

Modified PEEK Blends, Carbon Filled

PEEK-modified (25-30% carbon filled, wear grade)

PEEK-modified (30% carbon fiber)

PEEK-modified (45-55% carbon filled, wear grade, high load)