PEEK 30% Glass Fiber Material Data Sheet

PEEK 30% Glass Fiber (Polyetheretherketone) Material Data Sheet

PEEK 30% Glass Fiber Overview

PEEK 30% glass fiber is a grade of polyetheretherketone (PEEK), designated Polyetheretherketone (30% Glass Fiber). This PEEK 30% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PEEK parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PEEK parts in-house and inspects them before shipment.

PEEK Designation

Polyetheretherketone (30% Glass Fiber)
TradenamesDynamix, Edgetek, Gatone, Hifill, Kebapeak, Ketaspire, Ketron, Larpeek, LNP Thermocomp, Luvocom, Pyramid, Schulatec, Vestakeep, Victrex

PEEK Typical uses

Wire covering, injection molded engineering products, film for flexible pcb, resin in fiber prepegs, aerospace applications, radiation environments.

PEEK 30% Glass Fiber Composition detail

Polymer70  %
Glass (fiber)30  %

PEEK Physical properties

Density1.49–1.54g/cm3

PEEK 30% Glass Fiber Mechanical properties

Young’s modulus8.62–11GPa
Specific stiffness5.69–7.27MN.m/kg
Yield strength (elastic limit)124–158MPa
Tensile strength155–197MPa
Specific strength81.8–104kN.m/kg
Elongation2–3% strain
Compressive modulus8.62–11GPa
Compressive strength147–154MPa
Flexural modulus8.66–11GPa
Flexural strength (modulus of rupture)228–290MPa
Shear modulus3.18–4.06GPa
Bulk modulus10.9–11.5GPa
Poisson’s ratio0.39–0.41 
Shape factor6.5
Hardness – Vickers37–47HV
Hardness – Rockwell M98–108 
Hardness – Rockwell R120–132 
Elastic stored energy (springs)780–1290kJ/m3
Fatigue strength at 10^7 cycles61.7–80.3MPa

PEEK Impact & fracture properties

Fracture toughness5.34–7.93MPa.m0.5
Toughness (G)2.98–6.33kJ/m2
Impact strength, notched 23 °C9.09–11kJ/m2
Impact strength, notched -30 °C8.18–9.9kJ/m2
Impact strength, unnotched 23 °C63.6–77kJ/m2
Impact strength, unnotched -30 °C68.2–82.5kJ/m2

PEEK 30% Glass Fiber Thermal properties

Melting point322–346°C
Glass temperature143–157°C
Heat deflection temperature 0.45MPa306–356°C
Heat deflection temperature 1.8MPa288–315°C
Maximum service temperature260–280°C
Minimum service temperature-70–-50°C
Thermal conductivity0.197–0.213W/m.°C
Specific heat capacity1000–1100J/kg.°C
Thermal expansion coefficient20–30µstrain/°C
Thermal shock resistance455–755°C
Thermal distortion resistance0.00681–0.0103MW/m

PEEK Electrical properties

Electrical resistivity3300000000000000000000–30000000000000000000000µohm.cm
Electrical conductivity5.75e-21–5.22e-20%IACS
Dielectric constant (relative permittivity)3.2–3.4 
Dissipation factor (dielectric loss tangent)0.0019–0.0021 
Dielectric strength (dielectric breakdown)16.5–19.8MV/m
Comparative tracking index175–225V

PEEK Magnetic properties

Magnetic typeNon-magnetic

PEEK Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2380–2700m/s
Mechanical loss coefficient (tan delta)0.00747–0.00886 

PEEK Absorption & permeability

Water absorption @ 24 hrs0.06–0.12%

PEEK Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 1.4 %
Melt temperature305 – 399 °C
Mold temperature120 – 160 °C
Molding pressure range68.8 – 138 MPa

PEEK Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Excellent
FlammabilitySelf-extinguishing