Custom 450 ST Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)
Custom 450 ST Stainless Steel Overview
Custom 450 ST stainless steel is a martensitic precipitation hardening stainless steel (UNS S45000) in the wrought form. Condition: Solution annealed. This Custom 450 ST stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for Custom 450 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined Custom 450 parts in-house and inspects them before shipment.
Custom 450 Designation
Custom 450, wrought
Condition
Solution annealed
UNS number
S45000
US name
Custom 450
Custom 450 ST Stainless Steel Composition detail
C (carbon)
0
–
0.05
%
Cr (chromium)
14
–
16
%
Cu (copper)
1.25
–
1.75
%
Fe (iron)
72.1
–
79.2
%
Mn (manganese)
0
–
1
%
Mo (molybdenum)
0.5
–
1
%
Ni (nickel)
5
–
7
%
P (phosphorus)
0
–
0.03
%
S (sulfur)
0
–
0.03
%
Si (silicon)
0
–
1
%
Custom 450 Physical properties
Density
7.88
–
7.96
g/cm3
Custom 450 ST Stainless Steel Mechanical properties
Young’s modulus
193
–
203
GPa
Specific stiffness
24.4
–
25.6
MN.m/kg
Yield strength (elastic limit)
655
–
724
MPa
Tensile strength
862
–
953
MPa
Specific strength
82.7
–
91.5
kN.m/kg
Elongation
7
–
13
% strain
Compressive strength
986
–
1090
MPa
Flexural modulus
193
–
203
GPa
Flexural strength (modulus of rupture)
655
–
724
MPa
Shear modulus
77
–
81
GPa
Bulk modulus
153
–
161
GPa
Poisson’s ratio
0.29
–
0.302
Shape factor
34
Hardness – Vickers
282
–
302
HV
Hardness – Rockwell B
103
–
105
HRB
Hardness – Rockwell C
27
–
30
HRC
Hardness – Brinell
261
–
289
HB
Elastic stored energy (springs)
1080
–
1320
kJ/m3
Fatigue strength at 10^7 cycles
387
–
517
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
376
–
533
MPa
Custom 450 Impact & fracture properties
Fracture toughness
232
–
284
MPa.m0.5
Toughness (G)
275
–
404
kJ/m2
Custom 450 ST Stainless Steel Thermal properties
Melting point
1400
–
1440
°C
Maximum service temperature
382
–
427
°C
Minimum service temperature
-73
–
-43
°C
Thermal conductivity
18
–
19.5
W/m.°C
Specific heat capacity
490
–
510
J/kg.°C
Thermal expansion coefficient
10.6
–
11.2
µstrain/°C
Thermal shock resistance
301
–
340
°C
Thermal distortion resistance
1.64
–
1.8
MW/m
Latent heat of fusion
251
–
325
kJ/kg
Custom 450 Electrical properties
Electrical resistivity
98.2
–
100
µohm.cm
Electrical conductivity
1.72
–
1.76
%IACS
Galvanic potential
-0.22
–
-0.14
V
Custom 450 Magnetic properties
Magnetic type
Magnetic
Custom 450 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
4940
–
5060
m/s
Mechanical loss coefficient (tan delta)
3.1e-4
–
6.6e-4
Custom 450 Processing properties
Metal casting
Unsuitable
Metal cold forming
Limited use
Metal hot forming
Acceptable
Metal press forming
Acceptable
Metal deep drawing
Unsuitable
Machining speed
14.9 m/min
Weldability Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIG
Good
Weldability – plasma
Good
Weldability – SAW
Not recommended
Weldability – TIG
Good
Brazeability
Good
Carbon equivalency
0.625 – 0.892
Custom 450 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Excellent
Strong acids
Acceptable
Weak alkalis
Excellent
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Excellent
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Limited use
Flammability
Non-flammable
Custom 450 ST Stainless Steel Corrosion resistance
Pitting resistance equivalent number (PREN)
15.7 – 19.3
Pitting and crevice corrosion
Low (<20)
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Susceptible
Intergranular (weld line) corrosion
Good
Inorganic acids
Restricted
Organic acids
Moderate
Alkalis
Moderate
Humidity / water
Excellent
Sea water
Restricted
Sour oil and gas
Good
Custom 450 Standards with similar compositions
USA: S45000 to ASTM A564/A564M, S45000 to ASTM A693, S45000 to ASTM A705/A705M-95, S45000 to ASTM A959, UNS S45000