Custom 450 H1050 Stainless Steel Material Data Sheet

Custom 450 H1050 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)

Custom 450 H1050 Stainless Steel Overview

Custom 450 H1050 stainless steel is a martensitic precipitation hardening stainless steel (UNS S45000) in the wrought form. Condition: H1050 (Solution annealed; precipitation (age) hardened at 566°C; air cooled). This Custom 450 H1050 stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for Custom 450 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined Custom 450 parts in-house and inspects them before shipment.

Custom 450 Designation

Custom 450, wrought
ConditionH1050 (Solution annealed; precipitation (age) hardened at 566°C; air cooled)
UNS numberS45000
US nameCustom 450

Custom 450 Typical uses

Processing of potentially corrosive liquids e.g. chemicals/oil/beverages/sewage, structural uses in corrosive environments, e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes

Custom 450 H1050 Stainless Steel Composition detail

C (carbon)0–0.05%
Cr (chromium)14–16%
Cu (copper)1.25–1.75%
Fe (iron)72.1–79.2%
Mn (manganese)0–1%
Mo (molybdenum)0.5–1%
Ni (nickel)5–7%
P (phosphorus)0–0.03%
S (sulfur)0–0.03%
Si (silicon)0–1%

Custom 450 Physical properties

Density7.71–7.79g/cm3

Custom 450 H1050 Stainless Steel Mechanical properties

Young’s modulus200–210GPa
Specific stiffness25.8–27.1MN.m/kg
Yield strength (elastic limit)917–1010MPa
Tensile strength993–1100MPa
Specific strength118–131kN.m/kg
Elongation12–20% strain
Compressive strength972–1070MPa
Flexural modulus200–210GPa
Flexural strength (modulus of rupture)917–1010MPa
Shear modulus77–80.9GPa
Bulk modulus159–167GPa
Poisson’s ratio0.29–0.302 
Shape factor25
Hardness – Vickers370–390HV
Hardness – Rockwell B108–112HRB
Hardness – Rockwell C34–39HRC
Hardness – Brinell322–358HB
Elastic stored energy (springs)2050–2510kJ/m3
Fatigue strength at 10^7 cycles397–590MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
388–604MPa

Custom 450 Impact & fracture properties

Fracture toughness163–199MPa.m0.5
Toughness (G)130–192kJ/m2

Custom 450 H1050 Stainless Steel Thermal properties

Melting point1400–1440°C
Maximum service temperature382–427°C
Minimum service temperature-73–-43°C
Thermal conductivity18–19.5W/m.°C
Specific heat capacity490–510J/kg.°C
Thermal expansion coefficient11–11.6µstrain/°C
Thermal shock resistance392–443°C
Thermal distortion resistance1.58–1.74MW/m
Latent heat of fusion266–327kJ/kg

Custom 450 Electrical properties

Electrical resistivity74.8–76.8µohm.cm
Electrical conductivity2.24–2.3%IACS
Galvanic potential-0.22–-0.14V

Custom 450 Magnetic properties

Magnetic typeMagnetic

Custom 450 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5080–5210m/s
Mechanical loss coefficient (tan delta)3.1e-4–6.6e-4 

Custom 450 Processing properties

Metal castingUnsuitable
Metal cold formingLimited use
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingUnsuitable
Machining speed11.6 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIGGood
Weldability – plasmaGood
Weldability – SAWNot recommended
Weldability – TIGGood
BrazeabilityGood
Carbon equivalency0.625 – 0.892

Custom 450 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Limited use
FlammabilityNon-flammable

Custom 450 H1050 Stainless Steel Corrosion resistance

Pitting resistance equivalent number (PREN)15.7 – 19.3
Pitting and crevice corrosionLow (<20)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Susceptible
Intergranular (weld line) corrosionGood
Inorganic acidsRestricted
Organic acidsModerate
AlkalisModerate
Humidity / waterExcellent
Sea waterRestricted
Sour oil and gasGood

Custom 450 Notes

Custom 450 H1050 Warning
Check with supplier what tempering and aging procedure has been applied – it could make a major difference to the steel’s mechanical properties.

Custom 450 Standards with similar compositions

USA: S45000 to ASTM A564/A564M, S45000 to ASTM A693, S45000 to ASTM A705/A705M-95, S45000 to ASTM A959, UNS S45000
Tradenames: CUSTOM 450 STAINLESS