17-7PH TH1050 Stainless Steel Material Data Sheet (Semi-austenitic, Precipitation Hardened)
17-7PH TH1050 Stainless Steel Overview
17-7PH TH1050 stainless steel is a semi-austenitic precipitation hardening stainless steel (UNS S17700) in the wrought form. Condition: TH1050 (Solution annealed; precipitation (age) hardened at 566°C; air cooled). This 17-7PH TH1050 stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 17-7PH parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined 17-7PH parts in-house and inspects them before shipment.
17-7PH Designation
17-7PH, wrought
Condition
TH1050 (Solution annealed; precipitation (age) hardened at 566°C; air cooled)
UNS number
S17700
US name
~ASTM S17700, ~ASME 631, ~AMS 5529, ~AMS 5528
EN name
~X7CrNiAl17-7
EN number
~1.4568
ISO name
~X7CrNiAl17-7, ~X7CrNial17-7
JIS (Japanese) name
SUS631
17-7PH Typical uses
Processing of potentially corrosive liquids e.g. chemicals/oil/beverages/sewage, structural uses in corrosive environments, e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Susceptible
Intergranular (weld line) corrosion
Good
Inorganic acids
Restricted
Organic acids
Moderate
Alkalis
Moderate
Humidity / water
Excellent
Sea water
Restricted
Sour oil and gas
Restricted
17-7PH Standards with similar compositions
China: 0Cr17Ni7Al to GB 1220, 0Cr17Ni7Al to GB 1221, 0Cr17Ni7Al to GB 4237, 0Cr17Ni7Al to GB 4238, 0Cr17Ni7Al to GB/T 3280, 0Cr17Ni7Al to GB/T 4231, 0Cr17Ni7Al to GB/T 4239, 0Cr17Ni7Al to GB/T 4356, 0Cr17Ni7Al to GB/T 6725
France: Z8CNA17.07 to AFNOR NF A35-581
Germany: 1.4568 to DIN EN 10088
International: X7CrNiAl17-7 to ISO 16143-1, X7CrNial17-7 to ISO 16143-2, X7CrNiAl17-7 to ISO 16143-3, X7CrNiAl17-7 to ISO 6931-1, X7CrNiAl17-7 to ISO 6931-2
Japan: SUS631 to JIS G4303, SUS631 to JIS G4304, SUS631 to JIS G4305, SUS631 to JIS G4306, SUS631 to JIS G4307, SUS631-CSP to JIS G4313, SUS631J1 to JIS G4308
South Korea: STS 631 to KS D 3706, STS 631-CSP to KS D 3534, STS 631J1 to KS D 3535, STS631 to KS D 3698, STS631 to KS D 3705, STS631J1 to KS D 3702
Sweden: 2388 to SS 142388
UK: 301S81 to BS 2056, X7CrNiAl17-7 to BS EN 10088-1, X7CrNiAl17-7 to BS EN 10088-2, X7CrNiAl17-7 to BS EN 10088-3, X7CrNiAl17-7 to BS EN 10270-3
USA: 17-7 PH to MIL-S-25043, 17-7PH to SAE J467, 5528 to AMS 5528, 5529 to AMS 5529, 5568 to AMS 5568, 5644 to AMS 5644, 5673 to AMS 5673, 5678 to AMS 5678, 62 to ASTM A579, S17700 to ASTM A313/A313M, S17700 to ASTM A564/A564M, S17700 to ASTM A693, S17700 to ASTM A705/A705M-95, S17700 to ASTM A959, UNS S17700, UNS S17780