15-5PH Cast H935 Stainless Steel Material Data Sheet

15-5PH Cast H935 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)

15-5PH Cast H935 Overview

15-5PH cast H935 is a martensitic precipitation hardening stainless steel (UNS S15500) in the cast form. In the H935 condition it is solution annealed, then age hardened at 502°C and air cooled. This 15-5PH cast H935 material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 15-5PH castings from Turkey (Türkiye)? Modulus Metal supplies 15-5PH castings with in-house CNC machining and inspects them before shipment.

15-5PH Designation

15-5PH
ConditionH935 (Solution annealed; precipitation (age) hardened at 502°C; air cooled)
UNS numberS15500
US name15-5PH

15-5PH Cast H935 Composition detail

C (carbon)0–0.05%
Cr (chromium)14–15.5%
Cu (copper)2.5–3.2%
Fe (iron)74.2–78.6%
Mn (manganese)0–0.6%
N (nitrogen)0–0.05%
Nb (niobium)0.15–0.3%
Ni (nickel)4.2–5%
P (phosphorus)0–0.025%
S (sulfur)0–0.025%
Si (silicon)0.5–1%
Ta (tantalum)0–0.05%

15-5PH Physical properties

Density7.77–7.84g/cm3

15-5PH Cast H935 Mechanical properties

Young’s modulus197–207GPa
Specific stiffness25.2–26.5MN.m/kg
Yield strength (elastic limit)1030–1140MPa
Tensile strength1170–1300MPa
Specific strength132–146kN.m/kg
Elongation6–6.97% strain
Compressive strength1070–1180MPa
Flexural modulus197–207GPa
Flexural strength (modulus of rupture)1030–1140MPa
Shear modulus77–80.9GPa
Bulk modulus142–150GPa
Poisson’s ratio0.27–0.281 
Shape factor21
Hardness – Vickers250–460HV
Elastic stored energy (springs)2650–3230kJ/m3
Fatigue strength at 10^7 cycles364–542MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
357–552MPa

15-5PH Impact & fracture properties

Fracture toughness83.7–102MPa.m0.5
Toughness (G)35–51.4kJ/m2

15-5PH Cast H935 Thermal properties

Melting point1400–1440°C
Maximum service temperature282–316°C
Minimum service temperature-73–-43°C
Thermal conductivity18–19.5W/m.°C
Specific heat capacity440–458J/kg.°C
Thermal expansion coefficient12.5–13.1µstrain/°C
Thermal shock resistance395–446°C
Thermal distortion resistance1.39–1.53MW/m
Latent heat of fusion260–285kJ/kg

15-5PH Electrical properties

Electrical resistivity72–82µohm.cm
Electrical conductivity2.1–2.39%IACS
Galvanic potential-0.22–-0.14V

15-5PH Magnetic properties

Magnetic typeMagnetic

15-5PH Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5020–5150m/s
Mechanical loss coefficient (tan delta)3.1e-4–6.6e-4 

15-5PH Processing properties

Metal castingLimited use
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed12.2 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Carbon equivalency0.637 – 0.81

15-5PH Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

15-5PH Cast H935 Corrosion resistance

Pitting resistance equivalent number (PREN)14 – 16.3
Pitting and crevice corrosionLow (<20)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Not susceptible

15-5PH Standards with similar compositions

India: Grade 2 to IS 11758
USA: 5346 to AMS 5346B, 5347 to AMS 5347A, 5357 to AMS 5357A, CB7Cu-2 to ASTM A747/A747M