Home » Precipitation Hardened Stainless Steels » AM-350 SCT 850 Stainless Steel Material Data Sheet
AM-350 SCT 850 Stainless Steel Material Data Sheet (Semi-austenitic, Precipitation Hardened)
AM-350 SCT 850 Stainless Steel Overview
AM-350 SCT 850 stainless steel is a semi-austenitic precipitation hardening stainless steel (UNS S35000) in the wrought form. Condition: SCT 850 (Solution annealed; hardened by sub-zero cooling and tempering at 455°C). This AM-350 SCT 850 stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for AM-350 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AM-350 parts in-house and inspects them before shipment.
AM-350 Designation
AM-350, wrought Condition SCT 850 (Solution annealed; hardened by sub-zero cooling and tempering at 455°C) UNS number S35000 US name AM-350
AM-350 Typical uses
Processing of potentially corrosive liquids e.g. chemicals/oil/beverages/sewage, structural uses in corrosive environments, e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes
AM-350 SCT 850 Stainless Steel Composition detail
C (carbon) 0.07 – 0.11 % Cr (chromium) 16 – 17 % Fe (iron) 72.7 – 76.9 % Mn (manganese) 0.5 – 1.25 % Mo (molybdenum) 2.5 – 3.25 % N (nitrogen) 0.07 – 0.13 % Ni (nickel) 4 – 5 % P (phosphorus) 0 – 0.04 % S (sulfur) 0 – 0.03 % Si (silicon) 0 – 0.5 %
AM-350 Physical properties
AM-350 SCT 850 Stainless Steel Mechanical properties
Young’s modulus 200 – 210 GPa Specific stiffness 25.6 – 26.9 MN.m/kg Yield strength (elastic limit) 1010 – 1120 MPa Tensile strength 1260 – 1390 MPa Specific strength 130 – 144 kN.m/kg Elongation 10 – 11.6 % strain Compressive strength 1120 – 1240 MPa Flexural modulus 200 – 210 GPa Flexural strength (modulus of rupture) 1010 – 1120 MPa Shear modulus 76 – 79.9 GPa Bulk modulus 185 – 195 GPa Poisson’s ratio 0.32 – 0.333 Shape factor 22 Hardness – Vickers 300 – 410 HV Hardness – Rockwell B 114 – 117 HRB Hardness – Rockwell C 44 – 50 HRC Hardness – Brinell 421 – 466 HB Elastic stored energy (springs) 2510 – 3060 kJ/m3 Fatigue strength at 10^7 cycles 505 – 574 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 480 – 604 MPa
AM-350 Impact & fracture properties
Fracture toughness 44.1 – 53.9 MPa.m0.5 Toughness (G) 9.56 – 14.1 kJ/m2
AM-350 SCT 850 Stainless Steel Thermal properties
Melting point 1400 – 1440 °C Maximum service temperature 382 – 427 °C Minimum service temperature -73 – -43 °C Thermal conductivity 15.2 – 16.5 W/m.°C Specific heat capacity 490 – 510 J/kg.°C Thermal expansion coefficient 11.2 – 11.7 µstrain/°C Thermal shock resistance 428 – 483 °C Thermal distortion resistance 1.32 – 1.45 MW/m Latent heat of fusion 308 – 379 kJ/kg
AM-350 Electrical properties
Electrical resistivity 77 – 107 µohm.cm Electrical conductivity 1.62 – 2.24 %IACS Galvanic potential -0.2 – -0.12 V
AM-350 Magnetic properties
AM-350 Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 5060 – 5190 m/s Mechanical loss coefficient (tan delta) 3.1e-4 – 6.6e-4
AM-350 Processing properties
Metal casting Unsuitable Metal cold forming Limited use Metal hot forming Acceptable Metal press forming Acceptable Metal deep drawing Unsuitable Machining speed 11.3 m/min Weldability Notes: Preheating is not required, post weld heat treatment is required Good Weldability – MIG Good Weldability – plasma Good Weldability – SAW Not recommended Weldability – TIG Good Brazeability Good Carbon equivalency 0.853 – 1.04
AM-350 Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Excellent Strong acids Acceptable Weak alkalis Excellent Strong alkalis Limited use Organic solvents Excellent Oxidation at 500C Excellent UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling. Limited use Flammability Non-flammable
AM-350 SCT 850 Stainless Steel Corrosion resistance
Pitting resistance equivalent number (PREN) 25.4 – 29.8 Pitting and crevice corrosion Medium (20-30) Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide Susceptible Intergranular (weld line) corrosion Good Inorganic acids Restricted Organic acids Moderate Alkalis Moderate Humidity / water Excellent Sea water Restricted Sour oil and gas Restricted
AM-350 Notes
AM-350 SCT 850 Warning Check with supplier what tempering and aging procedure has been applied – it could make a major difference to the steel’s mechanical properties.
AM-350 Standards with similar compositions
USA: 5554 to AMS 5554C, AM-350 to SAE J467, S35000 to ASTM A693, S35000 to ASTM A959, UNS S35000, UNS S35080Tradenames: AM 350, AM-350, AM-355 WROUGHT, CRONIFER 1705 MON – ALLOY 350, MCKAY 350, SLATER AM350