Home » Precipitation Hardened Stainless Steels » Custom 450 H900 Stainless Steel Material Data Sheet
Custom 450 H900 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)
Custom 450 H900 Stainless Steel Overview
Custom 450 H900 stainless steel is a martensitic precipitation hardening stainless steel (UNS S45000) in the wrought form. Condition: H900 (Solution annealed; precipitation (age) hardened at 482°C; air cooled). This Custom 450 H900 stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for Custom 450 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined Custom 450 parts in-house and inspects them before shipment.
Custom 450 Designation
Custom 450, wrought Condition H900 (Solution annealed; precipitation (age) hardened at 482°C; air cooled) UNS number S45000 US name Custom 450
Custom 450 H900 Stainless Steel Composition detail
C (carbon) 0 – 0.05 % Cr (chromium) 14 – 16 % Cu (copper) 1.25 – 1.75 % Fe (iron) 72.1 – 79.2 % Mn (manganese) 0 – 1 % Mo (molybdenum) 0.5 – 1 % Ni (nickel) 5 – 7 % P (phosphorus) 0 – 0.03 % S (sulfur) 0 – 0.03 % Si (silicon) 0 – 1 %
Custom 450 Physical properties
Custom 450 H900 Stainless Steel Mechanical properties
Young’s modulus 200 – 210 GPa Specific stiffness 25.8 – 27.1 MN.m/kg Yield strength (elastic limit) 1160 – 1280 MPa Tensile strength 1230 – 1360 MPa Specific strength 149 – 165 kN.m/kg Elongation 8 – 14 % strain Compressive strength 1190 – 1320 MPa Flexural modulus 200 – 210 GPa Flexural strength (modulus of rupture) 1160 – 1280 MPa Shear modulus 77 – 80.9 GPa Bulk modulus 159 – 167 GPa Poisson’s ratio 0.29 – 0.302 Shape factor 19 Hardness – Vickers 383 – 433 HV Hardness – Rockwell B 111 – 115 HRB Hardness – Rockwell C 39 – 45 HRC Hardness – Brinell 370 – 410 HB Elastic stored energy (springs) 3270 – 4000 kJ/m3 Fatigue strength at 10^7 cycles 558 – 660 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 532 – 692 MPa
Custom 450 Impact & fracture properties
Fracture toughness 94.5 – 116 MPa.m0.5 Toughness (G) 43.9 – 64.5 kJ/m2
Custom 450 H900 Stainless Steel Thermal properties
Melting point 1400 – 1440 °C Maximum service temperature 382 – 427 °C Minimum service temperature -73 – -43 °C Thermal conductivity 18 – 19.5 W/m.°C Specific heat capacity 490 – 510 J/kg.°C Thermal expansion coefficient 10.9 – 11.4 µstrain/°C Thermal shock resistance 500 – 565 °C Thermal distortion resistance 1.6 – 1.76 MW/m Latent heat of fusion 266 – 327 kJ/kg
Custom 450 Electrical properties
Electrical resistivity 82.6 – 86.6 µohm.cm Electrical conductivity 1.99 – 2.09 %IACS Galvanic potential -0.22 – -0.14 V
Custom 450 Magnetic properties
Custom 450 Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 5080 – 5210 m/s Mechanical loss coefficient (tan delta) 3.1e-4 – 6.6e-4
Custom 450 Processing properties
Metal casting Unsuitable Metal cold forming Limited use Metal hot forming Acceptable Metal press forming Acceptable Metal deep drawing Unsuitable Machining speed 10.4 m/min Weldability Notes: Preheating is not required, post weld heat treatment is required Good Weldability – MIG Good Weldability – plasma Good Weldability – SAW Not recommended Weldability – TIG Good Brazeability Good Carbon equivalency 0.625 – 0.892
Custom 450 Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Excellent Strong acids Acceptable Weak alkalis Excellent Strong alkalis Limited use Organic solvents Excellent Oxidation at 500C Excellent UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Notes: Aging martensitic steels at a low temperature, around 480 °C, improves resistance. Acceptable Flammability Non-flammable
Custom 450 H900 Stainless Steel Corrosion resistance
Pitting resistance equivalent number (PREN) 15.7 – 19.3 Pitting and crevice corrosion Low (<20) Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide Susceptible Intergranular (weld line) corrosion Good Inorganic acids Restricted Organic acids Moderate Alkalis Moderate Humidity / water Excellent Sea water Restricted Sour oil and gas Good
Custom 450 Standards with similar compositions
USA: S45000 to ASTM A564/A564M, S45000 to ASTM A693, S45000 to ASTM A705/A705M-95, S45000 to ASTM A959, UNS S45000Tradenames: CUSTOM 450 STAINLESS