Custom 455 H1000 Stainless Steel Material Data Sheet

Custom 455 H1000 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)

Custom 455 H1000 Stainless Steel Overview

Custom 455 H1000 stainless steel is a martensitic precipitation hardening stainless steel (UNS S45500) in the wrought form. Condition: H1000 (Solution annealed; precipitation (age) hardened at 540°C; air cooled). This Custom 455 H1000 stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for Custom 455 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined Custom 455 parts in-house and inspects them before shipment.

Custom 455 Designation

Custom 455, wrought
ConditionH1000 (Solution annealed; precipitation (age) hardened at 540°C; air cooled)
UNS numberS45500
US nameCustom 455

Custom 455 Typical uses

Processing of potentially corrosive liquids e.g. chemicals/oil/beverages/sewage, structural uses in corrosive environments, e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes

Custom 455 H1000 Stainless Steel Composition detail

C (carbon)0–0.05%
Cr (chromium)11–12.5%
Cu (copper)1.5–2.5%
Fe (iron)72–79.1%
Mn (manganese)0–0.5%
Mo (molybdenum)0–0.5%
Nb (niobium)0.1–0.5%
Ni (nickel)7.5–9.5%
P (phosphorus)0–0.04%
S (sulfur)0–0.03%
Si (silicon)0–0.5%
Ti (titanium)0.8–1.4%

Custom 455 Physical properties

Density7.71–7.79g/cm3

Custom 455 H1000 Stainless Steel Mechanical properties

Young’s modulus199–209GPa
Specific stiffness25.7–27MN.m/kg
Yield strength (elastic limit)1280–1410MPa
Tensile strength1380–1520MPa
Specific strength165–182kN.m/kg
Elongation10–11.6% strain
Compressive strength1330–1470MPa
Flexural modulus199–209GPa
Flexural strength (modulus of rupture)1280–1410MPa
Shear modulus79–83.1GPa
Bulk modulus138–145GPa
Poisson’s ratio0.26–0.271 
Shape factor17
Hardness – Vickers412–462HV
Hardness – Rockwell B113–116HRB
Hardness – Rockwell C42–48HRC
Hardness – Brinell399–442HB
Elastic stored energy (springs)3990–4880kJ/m3
Fatigue strength at 10^7 cycles630–682MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
590–728MPa

Custom 455 Impact & fracture properties

Fracture toughness99–121MPa.m0.5
Toughness (G)48.4–71.2kJ/m2

Custom 455 H1000 Stainless Steel Thermal properties

Melting point1400–1440°C
Maximum service temperature382–427°C
Minimum service temperature-73–-43°C
Thermal conductivity18–19.5W/m.°C
Specific heat capacity490–510J/kg.°C
Thermal expansion coefficient10.6–11.2µstrain/°C
Thermal shock resistance568–642°C
Thermal distortion resistance1.64–1.8MW/m
Latent heat of fusion232–285kJ/kg

Custom 455 Electrical properties

Electrical resistivity74.8–76.8µohm.cm
Electrical conductivity2.24–2.3%IACS
Galvanic potential-0.27–-0.19V

Custom 455 Magnetic properties

Magnetic typeMagnetic

Custom 455 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5070–5200m/s
Mechanical loss coefficient (tan delta)3.1e-4–6.6e-4 

Custom 455 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingUnsuitable
Machining speed8.84 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIGGood
Weldability – plasmaGood
Weldability – SAWNot recommended
Weldability – TIGGood
BrazeabilityGood
Carbon equivalency0.542 – 0.775

Custom 455 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

Custom 455 H1000 Stainless Steel Corrosion resistance

Pitting resistance equivalent number (PREN)11 – 14.2
Pitting and crevice corrosionLow (<20)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Susceptible
Intergranular (weld line) corrosionGood
Inorganic acidsRestricted
Organic acidsRestricted
AlkalisModerate
Humidity / waterExcellent
Sea waterRestricted
Sour oil and gasGood

Custom 455 Notes

Custom 455 H1000 Warning
Check with supplier what tempering and aging procedure has been applied – it could make a major difference to the steel’s mechanical properties.

Custom 455 Standards with similar compositions

USA: 5578 to AMS 5578D, 5672 to AMS 5672B, S45500 to ASTM A959, S45503 to ASTM A959, UNS S45500, UNS S45503
Tradenames: CRONIFER 1208 TI – ALLOY 455, CUSTOM 455 STAINLESS