Home » PA (Polyamide / Nylon) » PA66 (Polyamide 66 / Nylon 66) » PA66 Glass Filled Grades » PA66 30-35% Glass Fiber Toughened Material Data Sheet
PA66 30-35% Glass Fiber Toughened (Polyamide 66) Material Data Sheet
PA66 30-35% Glass Fiber Toughened Overview
PA66 30-35% glass fiber toughened is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, 30-35% Glass Fiber, Toughened). This PA66 30-35% glass fiber toughened material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.
PA66 30-35% Glass Fiber Toughened Designation
Polyamide (Nylon) (Type 66, 30-35% Glass Fiber, Toughened) Tradenames Altech, Mapex, Plustek, Schulamid, Terez, Ultramid, Wellamid
PA66 30-35% Glass Fiber Toughened Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA66 30-35% Glass Fiber Toughened Composition detail
Polymer 50 – 67 % Impact modifier 3 – 15 % Glass (fiber) 30 – 35 %
PA66 30-35% Glass Fiber Toughened Physical properties
PA66 30-35% Glass Fiber Toughened Mechanical properties
Young’s modulus 5.45 – 6.8 GPa Specific stiffness 4.26 – 5.31 MN.m/kg Yield strength (elastic limit) 93.5 – 117 MPa Tensile strength 97.9 – 120 MPa Specific strength 73 – 91.4 kN.m/kg Elongation 6.56 – 9.44 % strain Elongation at yield 5.52 – 10.5 % strain Compressive modulus 5.82 – 6.43 GPa Compressive strength 124 – 137 MPa Flexural modulus 4.68 – 5.6 GPa Flexural strength (modulus of rupture) 120 – 147 MPa Shear modulus 2.2 – 2.31 GPa Shear strength 58.7 – 71.8 MPa Bulk modulus 6.93 – 7.66 GPa Poisson’s ratio 0.34 – 0.36 Shape factor 5.79 Hardness – Vickers 30 – 33 HV Hardness – Rockwell M 151 – 167 Hardness – Rockwell R 151 – 167 Hardness – Brinell 120 – 150 HB Hardness – Shore D 91 – 94 Elastic stored energy (springs) 711 – 1140 kJ/m3 Fatigue strength at 10^7 cycles 41.3 – 45.7 MPa
PA66 30-35% Glass Fiber Toughened Impact & fracture properties
Fracture toughness 4.41 – 4.88 MPa.m0.5 Toughness (G) 3.06 – 4.09 kJ/m2 Impact strength, notched 23 °C 17.2 – 33.3 kJ/m2 Impact strength, notched -30 °C 7.75 – 16.9 kJ/m2 Impact strength, unnotched 23 °C 80 – 118 kJ/m2 Impact strength, unnotched -30 °C 76 – 114 kJ/m2
PA66 30-35% Glass Fiber Toughened Thermal properties
Melting point 256 – 265 °C Glass temperature 54 – 66 °C Heat deflection temperature 0.45MPa 249 – 257 °C Heat deflection temperature 1.8MPa 230 – 243 °C Maximum service temperature 57 – 77 °C Minimum service temperature -81 – -71 °C Thermal conductivity 0.399 – 0.415 W/m.°C Specific heat capacity 1480 – 1540 J/kg.°C Thermal expansion coefficient 76 – 79 µstrain/°C Thermal shock resistance 190 – 259 °C Thermal distortion resistance 0.00511 – 0.0054 MW/m
PA66 30-35% Glass Fiber Toughened Electrical properties
Electrical resistivity 2e17 – 5e18 µohm.cm Electrical conductivity 3.45e-17 – 8.62e-16 %IACS Dielectric constant (relative permittivity) 7.72 – 10.9 Dissipation factor (dielectric loss tangent) 0.033 – 0.087 Dielectric strength (dielectric breakdown) 55.5 – 94.5 MV/m Comparative tracking index 500 – 650 V
PA66 30-35% Glass Fiber Toughened Magnetic properties
Magnetic type Non-magnetic
PA66 30-35% Glass Fiber Toughened Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 2060 – 2310 m/s Mechanical loss coefficient (tan delta) 0.0111 – 0.0123
PA66 30-35% Glass Fiber Toughened Absorption & permeability
Water absorption @ 24 hrs 0.47 – 0.76 % Water absorption @ sat 4.2 – 5.6 % Humidity absorption @ sat 1.2 – 1.7 %
PA66 30-35% Glass Fiber Toughened Processing properties
Polymer injection molding Limited use Polymer extrusion Limited use Polymer thermoforming Limited use Linear mold shrinkage 0.25 – 0.45 % Melt temperature 225 – 302 °C Mold temperature 40 – 60 °C Molding pressure range 68.8 – 138 MPa
PA66 30-35% Glass Fiber Toughened Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Unacceptable Strong acids Unacceptable Weak alkalis Acceptable Strong alkalis Acceptable Organic solvents Acceptable Oxidation at 500C Unacceptable UV radiation (sunlight) Poor Flammability Slow-burning
Modulus Metal Services
Manufacturing & Quality Services in Turkey