PA6 50% Long Glass Fiber Material Data Sheet

PA6 50% Long Glass Fiber (Polyamide 6) Material Data Sheet

PA6 50% Long Glass Fiber Overview

PA6 50% long glass fiber is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 50% Long Glass Fiber). This PA6 50% long glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.

PA6 50% Long Glass Fiber Designation

Polyamide (Nylon) (Type 6, 50% Long Glass Fiber)
TradenamesCelstran, Complet, LNP Verton, Onforce

PA6 50% Long Glass Fiber Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 50% Long Glass Fiber Composition detail

Polymer50  %
Glass (fiber)50  %

PA6 50% Long Glass Fiber Physical properties

Density1.54–1.57g/cm3

PA6 50% Long Glass Fiber Mechanical properties

Young’s modulus10.9–13.5GPa
Specific stiffness7.01–8.69MN.m/kg
Yield strength (elastic limit)151–189MPa
Tensile strength153–187MPa
Specific strength97.1–122kN.m/kg
Elongation1.72–2.48% strain
Elongation at yield1.45–2.75% strain
Compressive modulus11.6–12.8GPa
Compressive strength194–214MPa
Flexural modulus9.92–11.9GPa
Flexural strength (modulus of rupture)239–292MPa
Shear modulus4.37–4.6GPa
Shear strength91.8–112MPa
Bulk modulus13.8–15.3GPa
Poisson’s ratio0.34–0.36 
Shape factor6.58
Hardness – Vickers49–54HV
Hardness – Rockwell M184–204 
Hardness – Rockwell R184–204 
Hardness – Shore D98–102 
Elastic stored energy (springs)931–1490kJ/m3
Fatigue strength at 10^7 cycles64.6–71.4MPa

PA6 50% Long Glass Fiber Impact & fracture properties

Fracture toughness5.07–5.6MPa.m0.5
Toughness (G)2.03–2.7kJ/m2
Impact strength, notched 23 °C25.8–50.2kJ/m2
Impact strength, notched -30 °C8.82–19.2kJ/m2
Impact strength, unnotched 23 °C84.6–124kJ/m2
Impact strength, unnotched -30 °C70.8–106kJ/m2

PA6 50% Long Glass Fiber Thermal properties

Melting point210–230°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa215–264°C
Heat deflection temperature 1.8MPa190–237°C
Maximum service temperature90–130°C
Minimum service temperature-64–-54°C
Thermal conductivity0.579–0.603W/m.°C
Specific heat capacity1280–1330J/kg.°C
Thermal expansion coefficient29.2–29.8µstrain/°C
Thermal shock resistance406–550°C
Thermal distortion resistance0.0196–0.0205MW/m

PA6 50% Long Glass Fiber Electrical properties

Electrical resistivity2e17–5e18µohm.cm
Electrical conductivity3.45e-17–8.62e-16%IACS
Dielectric constant (relative permittivity)9.2–13 
Dissipation factor (dielectric loss tangent)0.116–0.305 
Dielectric strength (dielectric breakdown)28.6–48.8MV/m
Comparative tracking index500–550V

PA6 50% Long Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PA6 50% Long Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2640–2950m/s
Mechanical loss coefficient (tan delta)0.00761–0.00841 

PA6 50% Long Glass Fiber Absorption & permeability

Water absorption @ 24 hrs0.93–1.5%
Water absorption @ sat4.1–5.4%
Humidity absorption @ sat1.2–1.7%

PA6 50% Long Glass Fiber Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 0.8 %
Melt temperature202 – 282 °C
Mold temperature50 – 60 °C
Molding pressure range68.8 – 138 MPa

PA6 50% Long Glass Fiber Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning