Home » PA (Polyamide / Nylon) » PA6 (Polyamide 6 / Nylon 6) » PA6 Glass Filled Grades » PA6 50% Glass Fiber Material Data Sheet
PA6 50% Glass Fiber (Polyamide 6) Material Data Sheet
PA6 50% Glass Fiber Overview
PA6 50% glass fiber is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 50% Glass Fiber). This PA6 50% glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.
PA6 50% Glass Fiber Designation
Polyamide (Nylon) (Type 6, 50% Glass Fiber) Tradenames Akromid, Akulon, Akulon Ultraflow, Anjacom, Badamid, Bergamid, Bestnyl, Celstran, Chemlon, Domamid, Durethan, Grilon, Hifill, Niretan, Novamid, Nylaforce, Pentamid, Petlon R-Prime, Plustek, Polybest, Radilon, Scanamid, Schulamid, Slovamid, Staramide, Tarnamid, Technyl, Technyl Star, Technylstar, Terez, Ultramid, Vitamide, Wellamid
PA6 50% Glass Fiber Typical uses
Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.
PA6 50% Glass Fiber Composition detail
Polymer 50 % Glass (fiber) 50 %
PA6 50% Glass Fiber Physical properties
PA6 50% Glass Fiber Mechanical properties
Young’s modulus 9.5 – 11.8 GPa Specific stiffness 6.01 – 7.47 MN.m/kg Yield strength (elastic limit) 137 – 171 MPa Tensile strength 138 – 169 MPa Specific strength 86.7 – 108 kN.m/kg Elongation 3.47 – 4.99 % strain Elongation at yield 2.92 – 5.54 % strain Compressive modulus 10.1 – 11.2 GPa Compressive strength 175 – 194 MPa Flexural modulus 8.71 – 10.4 GPa Flexural strength (modulus of rupture) 201 – 246 MPa Shear modulus 3.83 – 4.02 GPa Shear strength 83.1 – 102 MPa Bulk modulus 12.1 – 13.3 GPa Poisson’s ratio 0.34 – 0.36 Shape factor 6.4 Hardness – Vickers 44 – 49 HV Hardness – Rockwell M 178 – 197 Hardness – Rockwell R 178 – 197 Hardness – Brinell 97 – 121 HB Hardness – Shore D 97 – 101 Elastic stored energy (springs) 877 – 1390 kJ/m3 Fatigue strength at 10^7 cycles 58.5 – 64.6 MPa
PA6 50% Glass Fiber Impact & fracture properties
Fracture toughness 4.94 – 5.45 MPa.m0.5 Toughness (G) 2.21 – 2.93 kJ/m2 Impact strength, notched 23 °C 17.3 – 33.5 kJ/m2 Impact strength, notched -30 °C 8.82 – 19.2 kJ/m2 Impact strength, unnotched 23 °C 84.6 – 124 kJ/m2 Impact strength, unnotched -30 °C 70.8 – 106 kJ/m2
PA6 50% Glass Fiber Thermal properties
Melting point 210 – 230 °C Glass temperature 44 – 56 °C Heat deflection temperature 0.45MPa 197 – 245 °C Heat deflection temperature 1.8MPa 192 – 239 °C Maximum service temperature 90 – 130 °C Minimum service temperature -64 – -54 °C Thermal conductivity 0.521 – 0.542 W/m.°C Specific heat capacity 1280 – 1330 J/kg.°C Thermal expansion coefficient 52.9 – 55.1 µstrain/°C Thermal shock resistance 230 – 312 °C Thermal distortion resistance 0.00957 – 0.0101 MW/m
PA6 50% Glass Fiber Electrical properties
Electrical resistivity 1.32e19 – 3.31e20 µohm.cm Electrical conductivity 5.21e-19 – 1.31e-17 %IACS Dielectric constant (relative permittivity) 9.2 – 13 Dissipation factor (dielectric loss tangent) 0.116 – 0.305 Dielectric strength (dielectric breakdown) 28.6 – 48.8 MV/m Comparative tracking index 450 – 600 V
PA6 50% Glass Fiber Magnetic properties
Magnetic type Non-magnetic
PA6 50% Glass Fiber Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 2450 – 2740 m/s Mechanical loss coefficient (tan delta) 0.00812 – 0.00898
PA6 50% Glass Fiber Absorption & permeability
Water absorption @ 24 hrs 0.93 – 1.5 % Water absorption @ sat 4.1 – 5.4 % Humidity absorption @ sat 1.2 – 1.7 %
PA6 50% Glass Fiber Processing properties
Polymer injection molding Limited use Polymer extrusion Limited use Polymer thermoforming Limited use Linear mold shrinkage 0.091 – 0.11 % Melt temperature 226 – 302 °C Mold temperature 50 – 60 °C Molding pressure range 68.8 – 138 MPa
PA6 50% Glass Fiber Durability
Water (fresh) Excellent Water (salt) Acceptable Weak acids Unacceptable Strong acids Unacceptable Weak alkalis Limited use Strong alkalis Limited use Organic solvents Acceptable Oxidation at 500C Unacceptable UV radiation (sunlight) Fair Flammability Slow-burning