PA6 40% Long Glass Fiber Material Data Sheet

PA6 40% Long Glass Fiber (Polyamide 6) Material Data Sheet

PA6 40% Long Glass Fiber Overview

PA6 40% long glass fiber is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 40% Long Glass Fiber). This PA6 40% long glass fiber material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.

PA6 40% Long Glass Fiber Designation

Polyamide (Nylon) (Type 6, 40% Long Glass Fiber)
TradenamesCelstran, Complet, Sepaz, Stranox

PA6 40% Long Glass Fiber Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 40% Long Glass Fiber Composition detail

Polymer60  %
Glass (fiber)40  %

PA6 40% Long Glass Fiber Physical properties

Density1.44–1.47g/cm3

PA6 40% Long Glass Fiber Mechanical properties

Young’s modulus8.28–10.3GPa
Specific stiffness5.69–7.08MN.m/kg
Yield strength (elastic limit)130–162MPa
Tensile strength131–161MPa
Specific strength89.3–111kN.m/kg
Elongation1.8–2.6% strain
Elongation at yield1.52–2.88% strain
Compressive modulus8.84–9.77GPa
Compressive strength166–184MPa
Flexural modulus7.83–9.37GPa
Flexural strength (modulus of rupture)212–259MPa
Shear modulus3.33–3.5GPa
Shear strength78.8–96.4MPa
Bulk modulus10.5–11.6GPa
Poisson’s ratio0.34–0.36 
Shape factor6.11
Hardness – Vickers42–46HV
Hardness – Rockwell M174–192 
Hardness – Rockwell R174–192 
Hardness – Shore D96–100 
Elastic stored energy (springs)905–1440kJ/m3
Fatigue strength at 10^7 cycles55.5–61.3MPa

PA6 40% Long Glass Fiber Impact & fracture properties

Fracture toughness4.8–5.3MPa.m0.5
Toughness (G)2.39–3.18kJ/m2
Impact strength, notched 23 °C21.8–42.2kJ/m2
Impact strength, notched -30 °C2.66–5.77kJ/m2
Impact strength, unnotched 23 °C51.6–75.9kJ/m2
Impact strength, unnotched -30 °C34.9–52.3kJ/m2

PA6 40% Long Glass Fiber Thermal properties

Melting point210–271°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa209–258°C
Heat deflection temperature 1.8MPa184–231°C
Maximum service temperature90–130°C
Minimum service temperature-64–-54°C
Thermal conductivity0.514–0.534W/m.°C
Specific heat capacity1340–1400J/kg.°C
Thermal expansion coefficient36.5–37.3µstrain/°C
Thermal shock resistance366–496°C
Thermal distortion resistance0.0139–0.0145MW/m

PA6 40% Long Glass Fiber Electrical properties

Electrical resistivity1.2e19–3e20µohm.cm
Electrical conductivity5.75e-19–1.44e-17%IACS
Dielectric constant (relative permittivity)9.63–13.6 
Dissipation factor (dielectric loss tangent)0.138–0.365 
Dielectric strength (dielectric breakdown)28.1–47.9MV/m
Comparative tracking index425–475V

PA6 40% Long Glass Fiber Magnetic properties

Magnetic typeNon-magnetic

PA6 40% Long Glass Fiber Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2380–2670m/s
Mechanical loss coefficient (tan delta)0.00857–0.00947 

PA6 40% Long Glass Fiber Absorption & permeability

Water absorption @ 24 hrs1.1–1.8%
Water absorption @ sat4.8–6.4%
Humidity absorption @ sat1.5–2%

PA6 40% Long Glass Fiber Processing properties

Polymer injection moldingAcceptable
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.2 – 1 %
Melt temperature198 – 288 °C
Mold temperature50 – 60 °C
Molding pressure range68.8 – 138 MPa

PA6 40% Long Glass Fiber Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning