PA6 30% Glass Fiber Impact Modified Material Data Sheet

PA6 30% Glass Fiber Impact Modified (Polyamide 6) Material Data Sheet

PA6 30% Glass Fiber Impact Modified Overview

PA6 30% glass fiber impact modified is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 30% Glass Fiber, Impact Modified). This PA6 30% glass fiber impact modified material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.

PA6 30% Glass Fiber Impact Modified Designation

Polyamide (Nylon) (Type 6, 30% Glass Fiber, Impact Modified)
TradenamesAkulon, Altech, Chemlon, Domamid, Durethan, Grilon, Mapex, Pentamid, Schulamid, Taromid, Tecomid, Terez, Ultramid, Vitamide, Zytel

PA6 30% Glass Fiber Impact Modified Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 30% Glass Fiber Impact Modified Composition detail

Polymer55–67%
Impact modifier3–15%
Glass (fiber)30  %

PA6 30% Glass Fiber Impact Modified Physical properties

Density1.29–1.31g/cm3

PA6 30% Glass Fiber Impact Modified Mechanical properties

Young’s modulus4.74–5.91GPa
Specific stiffness3.65–4.55MN.m/kg
Yield strength (elastic limit)88.7–111MPa
Tensile strength89.6–110MPa
Specific strength68.2–85.4kN.m/kg
Elongation6.35–9.14% strain
Elongation at yield5.34–10.1% strain
Compressive modulus5.06–5.59GPa
Compressive strength114–126MPa
Flexural modulus4.31–5.16GPa
Flexural strength (modulus of rupture)131–160MPa
Shear modulus1.91–2.01GPa
Shear strength53.8–65.7MPa
Bulk modulus6.02–6.65GPa
Poisson’s ratio0.34–0.36 
Shape factor5.51
Hardness – Vickers28–31HV
Hardness – Rockwell M145–160 
Hardness – Rockwell R145–160 
Hardness – Brinell71–89HB
Hardness – Shore D89–93 
Elastic stored energy (springs)736–1180kJ/m3
Fatigue strength at 10^7 cycles37.9–41.8MPa

PA6 30% Glass Fiber Impact Modified Impact & fracture properties

Fracture toughness4.29–4.74MPa.m0.5
Toughness (G)3.33–4.44kJ/m2
Impact strength, notched 23 °C22.1–42.8kJ/m2
Impact strength, notched -30 °C9.61–20.9kJ/m2
Impact strength, unnotched 23 °C82.7–121kJ/m2
Impact strength, unnotched -30 °C68–102kJ/m2

PA6 30% Glass Fiber Impact Modified Thermal properties

Melting point210–220°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa197–220°C
Heat deflection temperature 1.8MPa187–234°C
Maximum service temperature57–77°C
Minimum service temperature-64–-54°C
Thermal conductivity0.426–0.443W/m.°C
Specific heat capacity1430–1490J/kg.°C
Thermal expansion coefficient36–45µstrain/°C
Thermal shock resistance387–561°C
Thermal distortion resistance0.00964–0.0121MW/m

PA6 30% Glass Fiber Impact Modified Electrical properties

Electrical resistivity1.16e19–2.89e20µohm.cm
Electrical conductivity5.97e-19–1.49e-17%IACS
Dielectric constant (relative permittivity)10.1–14.2 
Dissipation factor (dielectric loss tangent)0.133–0.351 
Dielectric strength (dielectric breakdown)24.1–41MV/m
Comparative tracking index500–600V

PA6 30% Glass Fiber Impact Modified Magnetic properties

Magnetic typeNon-magnetic

PA6 30% Glass Fiber Impact Modified Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1910–2140m/s
Mechanical loss coefficient (tan delta)0.0116–0.0128 

PA6 30% Glass Fiber Impact Modified Absorption & permeability

Water absorption @ 24 hrs1.2–2%
Water absorption @ sat5.4–7.1%
Humidity absorption @ sat1.6–2.1%

PA6 30% Glass Fiber Impact Modified Processing properties

Polymer injection moldingExcellent
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.3 – 0.5 %
Melt temperature205 – 288 °C
Mold temperature50 – 60 °C
Molding pressure range20.6 – 138 MPa

PA6 30% Glass Fiber Impact Modified Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySlow-burning