PA6 30% Glass Fiber Flame Retarded Material Data Sheet

PA6 30% Glass Fiber Flame Retarded (Polyamide 6) Material Data Sheet

PA6 30% Glass Fiber Flame Retarded Overview

PA6 30% glass fiber flame retarded is a grade of polyamide 6 (PA6, nylon 6), designated Polyamide (Nylon) (Type 6, 30% Glass Fiber, Flame Retarded). This PA6 30% glass fiber flame retarded material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA6 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA6 parts in-house and inspects them before shipment.

PA6 30% Glass Fiber Flame Retarded Designation

Polyamide (Nylon) (Type 6, 30% Glass Fiber, Flame Retarded)
TradenamesAbel, Akulon, Akulon Ultraflow, Cheng, Dinalon, Domamid, Durethan, Eplamid, Frblend, Frianyl, Novamid, Nylfor, Radiflam, Schulamid, Slovamid, Tarnamid

PA6 30% Glass Fiber Flame Retarded Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA6 30% Glass Fiber Flame Retarded Composition detail

Polymer55–65%
Flame retardant5–15%
Glass (fiber)30  %

PA6 30% Glass Fiber Flame Retarded Physical properties

Density1.53–1.56g/cm3

PA6 30% Glass Fiber Flame Retarded Mechanical properties

Young’s modulus6.8–8.48GPa
Specific stiffness4.4–5.49MN.m/kg
Yield strength (elastic limit)71.2–88.8MPa
Tensile strength83.1–102MPa
Specific strength46.1–57.5kN.m/kg
Elongation2.87–4.13% strain
Elongation at yield2.42–4.59% strain
Compressive modulus7.26–8.03GPa
Compressive strength105–116MPa
Flexural modulus4.61–5.52GPa
Flexural strength (modulus of rupture)104–127MPa
Shear modulus2.74–2.88GPa
Shear strength49.9–61MPa
Bulk modulus8.64–9.55GPa
Poisson’s ratio0.34–0.36 
Shape factor7.9
Hardness – Vickers23–25HV
Hardness – Rockwell M139–154 
Hardness – Rockwell R139–154 
Hardness – Shore D88–91 
Elastic stored energy (springs)330–525kJ/m3
Fatigue strength at 10^7 cycles35.1–38.8MPa

PA6 30% Glass Fiber Flame Retarded Impact & fracture properties

Fracture toughness4.61–5.1MPa.m0.5
Toughness (G)2.68–3.58kJ/m2
Impact strength, notched 23 °C8.43–16.4kJ/m2
Impact strength, notched -30 °C6.72–14.6kJ/m2
Impact strength, unnotched 23 °C46.8–68.8kJ/m2
Impact strength, unnotched -30 °C37.3–56kJ/m2

PA6 30% Glass Fiber Flame Retarded Thermal properties

Melting point210–220°C
Glass temperature44–56°C
Heat deflection temperature 0.45MPa192–220°C
Heat deflection temperature 1.8MPa193–204°C
Maximum service temperature90–130°C
Minimum service temperature-64–-54°C
Thermal conductivity0.494–0.514W/m.°C
Specific heat capacity1220–1270J/kg.°C
Thermal expansion coefficient39.2–40µstrain/°C
Thermal shock resistance227–308°C
Thermal distortion resistance0.0125–0.013MW/m

PA6 30% Glass Fiber Flame Retarded Electrical properties

Electrical resistivity3.41e19–8.52e20µohm.cm
Electrical conductivity2.02e-19–5.06e-18%IACS
Dielectric constant (relative permittivity)7.47–10.5 
Dissipation factor (dielectric loss tangent)0.118–0.312 
Dielectric strength (dielectric breakdown)20–34MV/m
Comparative tracking index250–600V

PA6 30% Glass Fiber Flame Retarded Magnetic properties

Magnetic typeNon-magnetic

PA6 30% Glass Fiber Flame Retarded Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity2090–2350m/s
Mechanical loss coefficient (tan delta)0.0112–0.0123 

PA6 30% Glass Fiber Flame Retarded Absorption & permeability

Water absorption @ 24 hrs0.86–1.4%
Water absorption @ sat3.8–5%
Humidity absorption @ sat1.2–1.6%

PA6 30% Glass Fiber Flame Retarded Processing properties

Polymer injection moldingExcellent
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.091 – 0.11 %
Melt temperature217 – 293 °C
Mold temperature50 – 60 °C
Molding pressure range82.5 – 172 MPa

PA6 30% Glass Fiber Flame Retarded Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisLimited use
Strong alkalisLimited use
Organic solventsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySelf-extinguishing