Custom 450 ST Stainless Steel Material Data Sheet

Custom 450 ST Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)

Custom 450 ST Stainless Steel Overview

Custom 450 ST stainless steel is a martensitic precipitation hardening stainless steel (UNS S45000) in the wrought form. Condition: Solution annealed. This Custom 450 ST stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for Custom 450 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined Custom 450 parts in-house and inspects them before shipment.

Custom 450 Designation

Custom 450, wrought
ConditionSolution annealed
UNS numberS45000
US nameCustom 450

Custom 450 ST Stainless Steel Composition detail

C (carbon)0–0.05%
Cr (chromium)14–16%
Cu (copper)1.25–1.75%
Fe (iron)72.1–79.2%
Mn (manganese)0–1%
Mo (molybdenum)0.5–1%
Ni (nickel)5–7%
P (phosphorus)0–0.03%
S (sulfur)0–0.03%
Si (silicon)0–1%

Custom 450 Physical properties

Density7.88–7.96g/cm3

Custom 450 ST Stainless Steel Mechanical properties

Young’s modulus193–203GPa
Specific stiffness24.4–25.6MN.m/kg
Yield strength (elastic limit)655–724MPa
Tensile strength862–953MPa
Specific strength82.7–91.5kN.m/kg
Elongation7–13% strain
Compressive strength986–1090MPa
Flexural modulus193–203GPa
Flexural strength (modulus of rupture)655–724MPa
Shear modulus77–81GPa
Bulk modulus153–161GPa
Poisson’s ratio0.29–0.302 
Shape factor34
Hardness – Vickers282–302HV
Hardness – Rockwell B103–105HRB
Hardness – Rockwell C27–30HRC
Hardness – Brinell261–289HB
Elastic stored energy (springs)1080–1320kJ/m3
Fatigue strength at 10^7 cycles387–517MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
376–533MPa

Custom 450 Impact & fracture properties

Fracture toughness232–284MPa.m0.5
Toughness (G)275–404kJ/m2

Custom 450 ST Stainless Steel Thermal properties

Melting point1400–1440°C
Maximum service temperature382–427°C
Minimum service temperature-73–-43°C
Thermal conductivity18–19.5W/m.°C
Specific heat capacity490–510J/kg.°C
Thermal expansion coefficient10.6–11.2µstrain/°C
Thermal shock resistance301–340°C
Thermal distortion resistance1.64–1.8MW/m
Latent heat of fusion251–325kJ/kg

Custom 450 Electrical properties

Electrical resistivity98.2–100µohm.cm
Electrical conductivity1.72–1.76%IACS
Galvanic potential-0.22–-0.14V

Custom 450 Magnetic properties

Magnetic typeMagnetic

Custom 450 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity4940–5060m/s
Mechanical loss coefficient (tan delta)3.1e-4–6.6e-4 

Custom 450 Processing properties

Metal castingUnsuitable
Metal cold formingLimited use
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingUnsuitable
Machining speed14.9 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIGGood
Weldability – plasmaGood
Weldability – SAWNot recommended
Weldability – TIGGood
BrazeabilityGood
Carbon equivalency0.625 – 0.892

Custom 450 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Limited use
FlammabilityNon-flammable

Custom 450 ST Stainless Steel Corrosion resistance

Pitting resistance equivalent number (PREN)15.7 – 19.3
Pitting and crevice corrosionLow (<20)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Susceptible
Intergranular (weld line) corrosionGood
Inorganic acidsRestricted
Organic acidsModerate
AlkalisModerate
Humidity / waterExcellent
Sea waterRestricted
Sour oil and gasGood

Custom 450 Standards with similar compositions

USA: S45000 to ASTM A564/A564M, S45000 to ASTM A693, S45000 to ASTM A705/A705M-95, S45000 to ASTM A959, UNS S45000
Tradenames: CUSTOM 450 STAINLESS