Transparent PA Semi-Aromatic Type 6I/6T Amorphous Material Data Sheet

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Material Data Sheet

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Overview

Transparent PA semi-aromatic type 6I/6T amorphous is a grade of transparent polyamide (PA), designated Transparent polyamide (nylon) (Semi-aromatic type 6I/6T, amorphous). This transparent PA semi-aromatic type 6I/6T amorphous material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for transparent polyamide parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined transparent polyamide parts in-house and inspects them before shipment.

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Designation

Transparent polyamide (nylon) (Semi-aromatic type 6I/6T, amorphous)
TradenamesGrivory, Selar, Trogamid, Durethan

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Typical uses

High-voltage switch casings, cable glands, battery seals, keys and push buttons, terminal strips, filter cups, metering devices, inspection glasses, flowmeters, liquid-level indicators, valve blocks, guide rails, coil body, toothbrush handle

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Composition detail

Polymer100  %

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Physical properties

Density1.17–1.19g/cm3

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Mechanical properties

Young’s modulus2.94–3.66GPa
Specific stiffness2.49–3.1MN.m/kg
Yield strength (elastic limit)80.1–99.9MPa
Tensile strength101–124MPa
Specific strength67.9–84.7kN.m/kg
Elongation41–59% strain
Elongation at yield3.45–6.55% strain
Compressive modulus3.14–3.47GPa
Compressive strength128–142MPa
Flexural modulus3–3.6GPa
Flexural strength (modulus of rupture)146–178MPa
Shear modulus1.15–1.21GPa
Shear strength60.8–74.3MPa
Bulk modulus5.28–5.83GPa
Poisson’s ratio0.385–0.401 
Shape factor4.52
Hardness – Vickers26–28HV
Hardness – Rockwell M154–170 
Hardness – Rockwell R154–170 
Hardness – Shore D91–95 
Hardness – Shore A97–100 
Elastic stored energy (springs)968–1540kJ/m3
Fatigue strength at 10^7 cycles42.8–47.3MPa
Tear strength159–169N/mm

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Impact & fracture properties

Fracture toughness3.89–4.3MPa.m0.5
Toughness (G)4.42–5.89kJ/m2
Impact strength, notched 23 °C6.8–13.2kJ/m2
Impact strength, notched -30 °C6.3–13.7kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2
Impact strength, unnotched -30 °C590–600kJ/m2

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Thermal properties

Glass temperature120–130°C
Heat deflection temperature 0.45MPa115  °C
Heat deflection temperature 1.8MPa105  °C
Vicat softening point123–133°C
Maximum service temperature40–60°C
Minimum service temperature-49–-29°C
Thermal conductivity0.206–0.214W/m.°C
Specific heat capacity1400–1500J/kg.°C
Thermal expansion coefficient60–80µstrain/°C
Thermal shock resistance321–482°C
Thermal distortion resistance0.00262–0.0035MW/m

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Electrical properties

Electrical resistivity2e20–5e21µohm.cm
Electrical conductivity3.45e-20–8.62e-19%IACS
Dielectric constant (relative permittivity)3.82–5.38 
Dissipation factor (dielectric loss tangent)0.0264–0.0696 
Dielectric strength (dielectric breakdown)20.7–35.3MV/m
Comparative tracking index600  V

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Magnetic properties

Magnetic typeNon-magnetic

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Optical, aesthetic and acoustic properties

Refractive index1.56–1.57 
TransparencyTransparent
Acoustic velocity1580–1760m/s
Mechanical loss coefficient (tan delta)0.0138–0.0153 

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Absorption & permeability

Water absorption @ 24 hrs1.2–1.9%
Water absorption @ sat5.2–6.8%
Humidity absorption @ sat1.7–2.3%
Water vapor transmission0.776–1.04g.mm/m².day
Permeability (O2)32–42.8cm³.mm/m².day.atm

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Processing properties

Polymer injection moldingExcellent
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.35 – 0.45 %
Melt temperature260 – 300 °C
Mold temperature60 – 80 °C
Molding pressure range80 – 160 MPa

Transparent PA Semi-Aromatic Type 6I/6T Amorphous Durability

Water (fresh)Acceptable
Water (salt)Acceptable
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisUnacceptable
Organic solventsLimited use
Oxidation at 500CUnacceptable
UV radiation (sunlight)Fair
FlammabilitySelf-extinguishing