AISI 1040 Annealed vs As Rolled vs Normalized vs Oil vs Water Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 1040 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1040 medium carbon steel (UNS G10400) side by side for 13 conditions: annealed, as rolled, normalized, oil quenched & tempered at 205°C, oil quenched & tempered at 315°C, oil quenched & tempered at 425°C, oil quenched & tempered at 540°C, oil quenched & tempered at 650°C, water quenched & tempered at 205°C, water quenched & tempered at 315°C, water quenched & tempered at 425°C, water quenched & tempered at 540°C, water quenched & tempered at 650°C. All values are taken from the individual AISI 1040 material data sheets linked below.

AISI 1040 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)Machining speed (m/min)
Annealed315–390475–575143–17324–3633.5
As Rolled375–460565–690188–22820–3025.6
Normalized335–415530–650160–19522–3429.3
Oil Quenched & Tempered at 205°C530–655700–860240–29015–2320.1
Oil Quenched & Tempered at 315°C530–655700–860235–28516–2420.1
Oil Quenched & Tempered at 425°C495–610680–835220–27016–2621.3
Oil Quenched & Tempered at 540°C440–540645–795195–24020–3223.8
Oil Quenched & Tempered at 650°C385–480565–700180–22023–3526.2
Water Quenched & Tempered at 205°C595–730805–990465–56512–2011.9
Water Quenched & Tempered at 315°C580–715800–985400–49014–2213.4
Water Quenched & Tempered at 425°C565–700755–925320–39016–2615.8
Water Quenched & Tempered at 540°C530–655700–860250–30018–2819.5
Water Quenched & Tempered at 650°C455–550600–740188–22822–3425

AISI 1040 Differences Compared with Annealed

The table below shows how much each AISI 1040 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.

ConditionYield strengthTensile strengthHardnessElongation
As Rolled+18%+20%+32%-17%
Normalized+6%+12%+12%-7%
Oil Quenched & Tempered at 205°C+68%+49%+68%-37%
Oil Quenched & Tempered at 315°C+68%+49%+65%-33%
Oil Quenched & Tempered at 425°C+57%+44%+55%-30%
Oil Quenched & Tempered at 540°C+39%+37%+38%-13%
Oil Quenched & Tempered at 650°C+23%+20%+27%-3%
Water Quenched & Tempered at 205°C+88%+71%+226%-47%
Water Quenched & Tempered at 315°C+84%+70%+182%-40%
Water Quenched & Tempered at 425°C+79%+60%+125%-30%
Water Quenched & Tempered at 540°C+68%+49%+74%-23%
Water Quenched & Tempered at 650°C+43%+28%+32%-7%

AISI 1040 Oil Quenched vs Water Quenched

Water removes heat faster than oil, so water quenched AISI 1040 forms more martensite and comes out harder and stronger, but with a higher risk of distortion and quench cracking. The table compares AISI 1040 oil quenched and water quenched material tempered at the same temperature, and shows the difference of water quenching relative to oil quenching (mid-points).

Tempered atYield oil / water (MPa)Yield diff.Tensile oil / water (MPa)Tensile diff.Hardness oil / water (HV)Hardness diff.
205°C530–655 / 595–730+12%700–860 / 805–990+15%240–290 / 465–565+94%
315°C530–655 / 580–715+9%700–860 / 800–985+14%235–285 / 400–490+71%
425°C495–610 / 565–700+14%680–835 / 755–925+11%220–270 / 320–390+45%
540°C440–540 / 530–655+21%645–795 / 700–860+8%195–240 / 250–300+26%
650°C385–480 / 455–550+16%565–700 / 600–740+6%180–220 / 188–228+4%

AISI 1040 Strength and Hardness Charts

Oil quenched & tempered   Water quenched & tempered. Dark bar = minimum, light bar = maximum of the range.

AISI 1040 Yield strength by condition (MPa)Annealed315–390As Rolled375–460Normalized335–415OQ&T 205°C530–655WQ&T 205°C595–730OQ&T 315°C530–655WQ&T 315°C580–715OQ&T 425°C495–610WQ&T 425°C565–700OQ&T 540°C440–540WQ&T 540°C530–655OQ&T 650°C385–480WQ&T 650°C455–550
AISI 1040 Tensile strength by condition (MPa)Annealed475–575As Rolled565–690Normalized530–650OQ&T 205°C700–860WQ&T 205°C805–990OQ&T 315°C700–860WQ&T 315°C800–985OQ&T 425°C680–835WQ&T 425°C755–925OQ&T 540°C645–795WQ&T 540°C700–860OQ&T 650°C565–700WQ&T 650°C600–740
AISI 1040 Hardness by condition (HV)Annealed143–173As Rolled188–228Normalized160–195OQ&T 205°C240–290WQ&T 205°C465–565OQ&T 315°C235–285WQ&T 315°C400–490OQ&T 425°C220–270WQ&T 425°C320–390OQ&T 540°C195–240WQ&T 540°C250–300OQ&T 650°C180–220WQ&T 650°C188–228

AISI 1040 Heat Treatment Key Points

The highest tensile strength of AISI 1040 in these data sheets is reached in the water quenched & tempered at 205°C condition (805–990 MPa). The softest condition is annealed (143–173 HV), with a machining speed of 33.5 m/min, which is usually preferred for machining and forming. For oil quenched AISI 1040, raising the tempering temperature from 205°C to 650°C lowers hardness from 240–290 HV to 180–220 HV, trading strength for toughness and ductility. For water quenched AISI 1040, raising the tempering temperature from 205°C to 650°C lowers hardness from 465–565 HV to 188–228 HV, trading strength for toughness and ductility.

AISI 1040 Material Data Sheets

AISI 1040 Annealed | AISI 1040 As Rolled | AISI 1040 Normalized | AISI 1040 Oil Quenched & Tempered at 205°C | AISI 1040 Oil Quenched & Tempered at 315°C | AISI 1040 Oil Quenched & Tempered at 425°C | AISI 1040 Oil Quenched & Tempered at 540°C | AISI 1040 Oil Quenched & Tempered at 650°C | AISI 1040 Water Quenched & Tempered at 205°C | AISI 1040 Water Quenched & Tempered at 315°C | AISI 1040 Water Quenched & Tempered at 425°C | AISI 1040 Water Quenched & Tempered at 540°C | AISI 1040 Water Quenched & Tempered at 650°C | All AISI 1040 conditions

Looking for AISI 1040 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1040 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.