AISI 1141 as rolled is AISI 1141 resulfurized medium carbon steel (UNS G11410) in the as rolled condition. This AISI 1141 as rolled material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1141 conditions in our AISI 1141 yield, tensile and hardness comparison. See also the resulfurized free-machining steels comparison. Looking for AISI 1141 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1141 steel parts in-house and inspects them before shipment.
AISI 1141 As Rolled Designation
AISI 1141
Condition
As rolled
UNS number
G11410
US name
ASTM G11410, ASTM 1141 Class B, ASTM 1141 Class A, ASTM 1141
AISI 1141 As Rolled Typical uses
General construction, general mechanical engineering, automotive, tools, axles, gears, springs.
AISI 1141 As Rolled Composition detail
C (carbon)
0.37
–
0.45
%
Fe (iron)
97.7
–
98.2
%
Mn (manganese)
1.35
–
1.65
%
P (phosphorus)
0
–
0.04
%
S (sulfur)
0.08
–
0.13
%
AISI 1141 As Rolled Physical properties
Density
7.8
–
7.9
g/cm3
AISI 1141 As Rolled Mechanical properties
Young’s modulus
200
–
215
GPa
Specific stiffness
25.5
–
27.4
MN.m/kg
Yield strength (elastic limit)
320
–
395
MPa
Tensile strength
595
–
745
MPa
Specific strength
40.8
–
50.3
kN.m/kg
Elongation
17
–
27
% strain
Compressive strength
320
–
395
MPa
Flexural modulus
200
–
215
GPa
Flexural strength (modulus of rupture)
320
–
395
MPa
Shear modulus
77
–
84
GPa
Bulk modulus
155
–
175
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
57
Hardness – Vickers
180
–
220
HV
Elastic stored energy (springs)
249
–
373
kJ/m3
Fatigue strength at 10^7 cycles
297
–
349
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
256
–
405
MPa
AISI 1141 As Rolled Impact & fracture properties
Fracture toughness
57
–
92
MPa.m0.5
Toughness (G)
16.4
–
39
kJ/m2
AISI 1141 As Rolled Thermal properties
Melting point
1430
–
1510
°C
Maximum service temperature
322
–
350
°C
Minimum service temperature
-58
–
-28
°C
Thermal conductivity
48
–
53
W/m.°C
Specific heat capacity
440
–
480
J/kg.°C
Thermal expansion coefficient
12
–
13.5
µstrain/°C
Thermal shock resistance
119
–
152
°C
Thermal distortion resistance
3.67
–
4.28
MW/m
Latent heat of fusion
270
–
275
kJ/kg
AISI 1141 As Rolled Electrical properties
Electrical resistivity
16
–
19
µohm.cm
Electrical conductivity
9.07
–
10.8
%IACS
Galvanic potential
-0.52
–
-0.44
V
AISI 1141 As Rolled Magnetic properties
Magnetic type
Magnetic
AISI 1141 As Rolled Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5050
–
5240
m/s
Mechanical loss coefficient (tan delta)
7.7e-4
–
9.7e-4
AISI 1141 As Rolled Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Acceptable
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
30.5 m/min
Weldability Notes: Preheating and post weld heat treatments may be required
Poor
Carbon equivalency
0.595 – 0.725
AISI 1141 As Rolled Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
Flammability
Non-flammable
AISI 1141 As Rolled Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Not susceptible
AISI 1141 As Rolled Standards with similar compositions
Argentina: IRAM 1141 to IAS
India: 40C15S12 to IS 1570/3, 40C15S12 to IS 9175/13, 40Mn15S12 to IS 3930, 40Mn2S12 to IS 1570/3
Italy: 40SMnPb10 to UNI 4838
Japan: SUM42 to JIS G4804
Mexico: 1139 to NMX-B-301, 1141 to NMX-B-301
Pan America: 1041 to COPANT 333, 1141 to COPANT 330, 1141 to COPANT 331, 1141 to COPANT 332, 1141 to COPANT 514
USA: 1139, 1139 to ASTM A29/A29M, 1139 to SAE J1249, 1141, 1141 Class A to ASTM A311/A311M, 1141 Class B to ASTM A311/A311M, 1141 to ASTM A29/A29M, 1141 to ASTM A519, 1141 to FED QQ-S-633A, 1141 to FED QQ-S-637A, 1141 to SAE J403, C1139 to FED QQ-S-637A, G11390 to ASTM A510/A510M, G11390 to ASTM A576-90b, G11410 to ASTM A510/A510M, G11410 to ASTM A576-90b, UNS G11390, UNS G11410