AISI 1030 Water Quenched & Tempered at 650°C Material Data Sheet

AISI 1030 Water Quenched & Tempered at 650°C Material Data Sheet

AISI 1030 Water Quenched & Tempered at 650°C Overview

AISI 1030 water quenched tempered 650°C is AISI 1030 medium carbon steel (UNS G10300) in the water quenched & tempered at 650°C condition. This AISI 1030 water quenched tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1030 conditions in our AISI 1030 yield, tensile and hardness comparison. Looking for AISI 1030 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1030 steel parts in-house and inspects them before shipment.

AISI 1030 Water Quenched & Tempered at 650°C Designation

AISI 1030
ConditionTempered at 650°C & water quenched
UNS numberG10300
US nameASTM 1030, ASTM 1029, ASTM G10290, ASME G10300, ~ASTM M1031, ~ASTM FPB, ~ASTM C2, ~ASTM A-1, ~ASTM 36, ~ASTM 1029, ~ASME G10290
JIS (Japanese) name~STPG 410, ~STKM15C, ~STKM15A, ~STKM14C, ~STKM14B, ~STKM14A, ~SPHT 4

AISI 1030 Water Quenched & Tempered at 650°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 1030 Water Quenched & Tempered at 650°C Composition detail

C (carbon)0.28–0.34%
Fe (iron)98.7–99.1%
Mn (manganese)0.6–0.9%
P (phosphorus)0–0.04%
S (sulfur)0–0.05%

AISI 1030 Water Quenched & Tempered at 650°C Physical properties

Density7.8–7.9g/cm3

AISI 1030 Water Quenched & Tempered at 650°C Mechanical properties

Young’s modulus208–216GPa
Specific stiffness26.5–27.5MN.m/kg
Yield strength (elastic limit)395–490MPa
Tensile strength525–650MPa
Specific strength50.3–62.4kN.m/kg
Elongation25–39% strain
Compressive strength395–490MPa
Flexural modulus208–216GPa
Flexural strength (modulus of rupture)395–490MPa
Shear modulus80–85GPa
Bulk modulus161–176GPa
Poisson’s ratio0.285–0.295 
Shape factor52
Hardness – Vickers190–230HV
Elastic stored energy (springs)372–561kJ/m3
Fatigue strength at 10^7 cycles272–317MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
235–367MPa

AISI 1030 Water Quenched & Tempered at 650°C Impact & fracture properties

Fracture toughness38–63MPa.m0.5
Toughness (G)7.17–17.8kJ/m2

AISI 1030 Water Quenched & Tempered at 650°C Thermal properties

Melting point1450–1510°C
Maximum service temperature331–353°C
Minimum service temperature-58–-33°C
Thermal conductivity50–55W/m.°C
Specific heat capacity465–505J/kg.°C
Thermal expansion coefficient11–12.5µstrain/°C
Thermal shock resistance156–201°C
Thermal distortion resistance4.13–4.84MW/m
Latent heat of fusion270–275kJ/kg

AISI 1030 Water Quenched & Tempered at 650°C Electrical properties

Electrical resistivity16–19µohm.cm
Electrical conductivity9.07–10.8%IACS
Galvanic potential-0.52–-0.44V

AISI 1030 Water Quenched & Tempered at 650°C Magnetic properties

Magnetic typeMagnetic

AISI 1030 Water Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5140–5250m/s
Mechanical loss coefficient (tan delta)7.4e-4–9.3e-4 

AISI 1030 Water Quenched & Tempered at 650°C Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingAcceptable
Machining speed26.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.38 – 0.49

AISI 1030 Water Quenched & Tempered at 650°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Limited use
FlammabilityNon-flammable

AISI 1030 Water Quenched & Tempered at 650°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Not susceptible

AISI 1030 Water Quenched & Tempered at 650°C Standards with similar compositions

China: ML30Mn to GB/T 6478
India: 30C8 to IS 1570/2/1, 35C8 to IS 1570/2/1, C30 to IS 1570/2/1, C30 to IS 6967, C35Mn75 to IS 1570/2/1, CDS-4 to IS 3074
Mexico: 1029 to NMX-B-301, 1030 to NMX-B-201, 1030 to NMX-B-203-SCFI, 1030 to NMX-B-301, 1034 to NMX-B-301, 1035 to NMX-B-203-SCFI, 1035 to NMX-B-301, 1037 to NMX-B-301
Pan America: 1029 to COPANT 333, 1030 to COPANT 330, 1030 to COPANT 331, 1030 to COPANT 333, 1034 to COPANT 333, 1035 to COPANT 330, 1035 to COPANT 331, 1035 to COPANT 333
Sweden: 1550 to SS 141550
UK: 080M30 to BS 970/1
USA: 1029, 1029 to ASTM A29/A29M, 1029 to SAE J403, 1030, 1030 to ASTM A29/A29M, 1030 to ASTM A512-96, 1030 to ASTM A513, 1030 to ASTM A519, 1030 to ASTM A568/A568M, 1030 to SAE J403, 1033, 1033 to ASTM A513, 1033 to ASTM A568/A568M, 1033 to SAE J403, 1034, 1034 to ASTM A29/A29M, 1035, 1035 Class A to ASTM A311/A311M, 1035 to ASTM A29/A29M, 1035 to ASTM A512-96, 1035 to ASTM A513, 1035 to ASTM A519, 1035 to ASTM A568/A568M, 1035 to DoD-F-24669/1, 1035 to FED QQ-W-461H, 1035 to SAE J403, 1037, 1037 to ASTM A29/A29M, 1037 to ASTM A568/A568M, 1037 to SAE J1249, 1037 to SAE J403, C1030 to FED QQ-S-635B, C1030 to FED QQ-S-700D, C1035 to FED QQ-S-635B, C1035 to FED QQ-S-700D, C3 to MIL-S-16788A, CS1030 to MIL-S-11310E, E to MIL-T-20157, G10290 to ASTM A510/A510M, G10290 to ASTM A576-90b, G10300 to ASTM A510/A510M, G10300 to ASTM A576-90b, G10300 to ASTM A830/A830M, G10330 to ASTM A830/A830M, G10340 to ASTM A510/A510M, G10350 to ASTM A510/A510M, G10350 to ASTM A576-90b, G10350 to ASTM A830/A830M, G10370 to ASTM A510/A510M, G10370 to ASTM A576-90b, G10370 to ASTM A830/A830M, MIL-S-3289B to MIL-S-3289B, UNS G10290, UNS G10300, UNS G10300 to UNS, UNS G10330, UNS G10340, UNS G10350, UNS G10350 to UNS, UNS G10370, UNS G10370 to UNS, UNS K02901
Tradenames: CS1030, D-M-E NO. 1, GREDE 34, JESSOP STEEL A-4 (S M-30), NITRIX 1473, V3, V3/1