AISI 1030 Annealed vs As Rolled vs Normalized vs Water Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 1030 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1030 medium carbon steel (UNS G10300) side by side for 8 conditions: annealed, as rolled, normalized, water quenched & tempered at 205°C, water quenched & tempered at 315°C, water quenched & tempered at 425°C, water quenched & tempered at 540°C, water quenched & tempered at 650°C. All values are taken from the individual AISI 1030 material data sheets linked below.

AISI 1030 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)Machining speed (m/min)
Annealed305–375410–515120–14525–3839.6
As Rolled310–380495–610170–20025–3929.6
Normalized310–380465–580143–17325–3933.5
Water Quenched & Tempered at 205°C580–715760–935450–55013–2112.5
Water Quenched & Tempered at 315°C555–685720–880360–44015–2314.9
Water Quenched & Tempered at 425°C520–640655–810275–35518–2818.3
Water Quenched & Tempered at 540°C460–575600–740235–28522–3421.6
Water Quenched & Tempered at 650°C395–490525–650190–23025–3926.5

AISI 1030 Differences Compared with Annealed

The table below shows how much each AISI 1030 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.

ConditionYield strengthTensile strengthHardnessElongation
As Rolled+1%+19%+40%+2%
Normalized+1%+13%+19%+2%
Water Quenched & Tempered at 205°C+90%+83%+277%-46%
Water Quenched & Tempered at 315°C+82%+73%+202%-40%
Water Quenched & Tempered at 425°C+71%+58%+138%-27%
Water Quenched & Tempered at 540°C+52%+45%+96%-11%
Water Quenched & Tempered at 650°C+30%+27%+58%+2%

AISI 1030 Strength and Hardness Charts

AISI 1030 Yield strength by condition (MPa)Annealed305–375As Rolled310–380Normalized310–380WQ&T 205°C580–715WQ&T 315°C555–685WQ&T 425°C520–640WQ&T 540°C460–575WQ&T 650°C395–490
AISI 1030 Tensile strength by condition (MPa)Annealed410–515As Rolled495–610Normalized465–580WQ&T 205°C760–935WQ&T 315°C720–880WQ&T 425°C655–810WQ&T 540°C600–740WQ&T 650°C525–650
AISI 1030 Hardness by condition (HV)Annealed120–145As Rolled170–200Normalized143–173WQ&T 205°C450–550WQ&T 315°C360–440WQ&T 425°C275–355WQ&T 540°C235–285WQ&T 650°C190–230

AISI 1030 Heat Treatment Key Points

The highest tensile strength of AISI 1030 in these data sheets is reached in the water quenched & tempered at 205°C condition (760–935 MPa). The softest condition is annealed (120–145 HV), with a machining speed of 39.6 m/min, which is usually preferred for machining and forming. For water quenched AISI 1030, raising the tempering temperature from 205°C to 650°C lowers hardness from 450–550 HV to 190–230 HV, trading strength for toughness and ductility.

AISI 1030 Material Data Sheets

AISI 1030 Annealed | AISI 1030 As Rolled | AISI 1030 Normalized | AISI 1030 Water Quenched & Tempered at 205°C | AISI 1030 Water Quenched & Tempered at 315°C | AISI 1030 Water Quenched & Tempered at 425°C | AISI 1030 Water Quenched & Tempered at 540°C | AISI 1030 Water Quenched & Tempered at 650°C | All AISI 1030 conditions