PA66 Lubricated 5% Silicone Material Data Sheet

PA66 Lubricated 5% Silicone (Polyamide 66) Material Data Sheet

PA66 Lubricated 5% Silicone Overview

PA66 lubricated 5% silicone is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, Lubricated, 5% Silicone). This PA66 lubricated 5% silicone material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 Lubricated 5% Silicone Designation

Polyamide (Nylon) (Type 66, Lubricated, 5% Silicone)
TradenamesAlcom, Ashlene, Bestnyl, Chemlon, Clariant, Delta, Eplamid, Hifill, Hylon, Hyundai, Latilub, LNP Lubricomp, LNP Lubriloy, Lubemid, Lubricomp, Lubrione, Luvocom, Nilamid, Nymax, Nypol, Oxnilon, Plaslube, Plustek, Polynil, Pryme, Radici, Spartech, Terez, Torzen, Tribocomp, Trimid, Vydyne, Zytel

PA66 Lubricated 5% Silicone Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA66 Lubricated 5% Silicone Composition detail

Polymer95  %
Silicone (lubricant)5  %

PA66 Lubricated 5% Silicone Physical properties

Density1.11–1.14g/cm3

PA66 Lubricated 5% Silicone Mechanical properties

Young’s modulus1.17–1.46GPa
Specific stiffness1.04–1.3MN.m/kg
Yield strength (elastic limit)37.8–47.1MPa
Tensile strength45.9–56.1MPa
Specific strength33.6–41.9kN.m/kg
Elongation25.3–36.3% strain
Elongation at yield11.7–22.2% strain
Compressive modulus1.25–1.38GPa
Compressive strength58.1–64.2MPa
Flexural modulus0.99–1.19GPa
Flexural strength (modulus of rupture)45–55.1MPa
Shear modulus0.455–0.478GPa
Shear strength27.5–33.6MPa
Bulk modulus2.34–2.59GPa
Poisson’s ratio0.395–0.411 
Shape factor4.18
Hardness – Vickers12–13HV
Hardness – Rockwell M101–112 
Hardness – Rockwell R101–112 
Hardness – Shore D77–80 
Elastic stored energy (springs)540–858kJ/m3
Fatigue strength at 10^7 cycles19.4–21.4MPa

PA66 Lubricated 5% Silicone Impact & fracture properties

Fracture toughness3.23–3.57MPa.m0.5
Toughness (G)7.63–10.2kJ/m2
Impact strength, notched 23 °C6.4–10kJ/m2
Impact strength, notched -30 °C3.3–7.18kJ/m2
Impact strength, unnotched 23 °C590–600kJ/m2
Impact strength, unnotched -30 °C590–600kJ/m2

PA66 Lubricated 5% Silicone Thermal properties

Melting point260–265°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa85–121°C
Heat deflection temperature 1.8MPa60–94°C
Maximum service temperature90–130°C
Minimum service temperature-81–-71°C
Thermal conductivity0.25–0.26W/m.°C
Specific heat capacity1570–1630J/kg.°C
Thermal expansion coefficient61.7–64.3µstrain/°C
Thermal shock resistance439–598°C
Thermal distortion resistance0.00393–0.00416MW/m

PA66 Lubricated 5% Silicone Electrical properties

Electrical resistivity5.37e19–1.34e21µohm.cm
Electrical conductivity1.29e-19–3.21e-18%IACS
Dielectric constant (relative permittivity)5.55–7.82 
Dissipation factor (dielectric loss tangent)0.0684–0.18 
Dielectric strength (dielectric breakdown)32.3–55MV/m
Comparative tracking index600  V

PA66 Lubricated 5% Silicone Magnetic properties

Magnetic typeNon-magnetic

PA66 Lubricated 5% Silicone Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1020–1140m/s
Mechanical loss coefficient (tan delta)0.0241–0.0266 

PA66 Lubricated 5% Silicone Absorption & permeability

Water absorption @ 24 hrs0.58–0.95%
Water absorption @ sat6.3–8.4%
Humidity absorption @ sat1.8–2.5%

PA66 Lubricated 5% Silicone Processing properties

Polymer injection moldingLimited use
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage1.36 – 1.65 %
Melt temperature223 – 299 °C
Molding pressure range6.88 – 103 MPa

PA66 Lubricated 5% Silicone Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySlow-burning