PA66 Molding Grade (Polyamide 66) Material Data Sheet
PA66 Molding Grade Overview
| PA66 molding grade is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, Molding). This PA66 molding grade material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment. |
PA66 Molding Grade Designation
| Polyamide (Nylon) (Type 66, Molding) | |
| Tradenames | Addinyl, Adell, Akromid, Akulon, Alcom, Altech, Amilan, Anjamid, Ashlene, Astamid, Badamid, Bergamid, Bestnyl, Chemlon, Chiao, Compamid, Dartek, Denyl, Deslon, Dinalon, Domamid, Ductel, Durethan, Dynacom, Eplamid, Germamid, Glamide, Grilon, Heramid, Hifill, Hylon, Hylonselect, Kopa, Latamid, Leona, Luvocom, Miramid, Next Industrial, Next Prime, Nilamid, Niretan, Novamid, Novamide, Nybex, Nycal, Nylaforce, Nylamid, Nylene, Nylfor, Nymax, Nypol, Omnilon, Opnyl, Pampellonne, Pentamid, Plaslube, Plustek, Polifil, Polybest, Polynil, Pryme, Quadrant, Radiflam, Radilon, Scanamid, Schulamid, Slovamid, Stabamid, Staramide, Star-Therm, Taromid, Technyl, Technyl Star, Tekamid, Terez, Therma-Tech, Thermylon, Torzen, Tribocomp, Trimid, Tufnyl, Ultramid, Unitika, Venyl, Vitamide, Vydyne, Wellamid, Zytel |
PA66 Molding Grade Typical uses
| Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils. |
PA66 Molding Grade Composition detail
| Polymer | 100 | % |
PA66 Molding Grade Physical properties
| Density | 1.13 | – | 1.15 | g/cm3 |
PA66 Molding Grade Mechanical properties
| Young’s modulus | 1.33 | – | 1.65 | GPa |
| Specific stiffness | 1.17 | – | 1.45 | MN.m/kg |
| Yield strength (elastic limit) | 51.1 | – | 63.8 | MPa |
| Tensile strength | 58.5 | – | 71.5 | MPa |
| Specific strength | 44.8 | – | 56 | kN.m/kg |
| Elongation | 41.8 | – | 60.2 | % strain |
| Elongation at yield | 14.6 | – | 27.8 | % strain |
| Compressive modulus | 1.41 | – | 1.56 | GPa |
| Compressive strength | 74.1 | – | 81.9 | MPa |
| Flexural modulus | 1.27 | – | 1.53 | GPa |
| Flexural strength (modulus of rupture) | 87 | – | 106 | MPa |
| Shear modulus | 0.511 | – | 0.537 | GPa |
| Shear strength | 35.1 | – | 42.9 | MPa |
| Bulk modulus | 2.95 | – | 3.26 | GPa |
| Poisson’s ratio | 0.4 | – | 0.42 | |
| Shape factor | 3.9 | |||
| Hardness – Vickers | 16 | – | 18 | HV |
| Hardness – Rockwell M | 58 | – | 65 | |
| Hardness – Rockwell R | 106 | – | 118 | |
| Hardness – Brinell | 64 | – | 80 | HB |
| Hardness – Shore D | 82 | – | 85 | |
| Elastic stored energy (springs) | 873 | – | 1390 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 24.7 | – | 27.3 | MPa |
PA66 Molding Grade Impact & fracture properties
| Fracture toughness | 3.32 | – | 3.66 | MPa.m0.5 |
| Toughness (G) | 7.12 | – | 9.44 | kJ/m2 |
| Impact strength, notched 23 °C | 10.8 | – | 20.9 | kJ/m2 |
| Impact strength, notched -30 °C | 3.29 | – | 7.16 | kJ/m2 |
| Impact strength, unnotched 23 °C | 590 | – | 600 | kJ/m2 |
| Impact strength, unnotched -30 °C | 590 | – | 600 | kJ/m2 |
PA66 Molding Grade Thermal properties
| Melting point | 255 | – | 265 | °C |
| Glass temperature | 54 | – | 66 | °C |
| Heat deflection temperature 0.45MPa | 218 | – | 246 | °C |
| Heat deflection temperature 1.8MPa | 70 | – | 100 | °C |
| Maximum service temperature | 90 | – | 130 | °C |
| Minimum service temperature | -81 | – | -71 | °C |
| Thermal conductivity | 0.233 | – | 0.253 | W/m.°C |
| Specific heat capacity | 1460 | – | 1580 | J/kg.°C |
| Thermal expansion coefficient | 110 | – | 150 | µstrain/°C |
| Thermal shock resistance | 243 | – | 370 | °C |
| Thermal distortion resistance | 0.00161 | – | 0.00222 | MW/m |
PA66 Molding Grade Electrical properties
| Electrical resistivity | 4.15e19 | – | 1.04e21 | µohm.cm |
| Electrical conductivity | 1.66e-19 | – | 4.15e-18 | %IACS |
| Dielectric constant (relative permittivity) | 6.8 | – | 9.58 | |
| Dissipation factor (dielectric loss tangent) | 0.0891 | – | 0.235 | |
| Dielectric strength (dielectric breakdown) | 20.8 | – | 35.4 | MV/m |
| Comparative tracking index | 500 | – | 600 | V |
PA66 Molding Grade Magnetic properties
| Magnetic type | Non-magnetic |
PA66 Molding Grade Optical, aesthetic and acoustic properties
| Refractive index | 1.52 | – | 1.56 | |
| Transparency | Translucent | |||
| Acoustic velocity | 1080 | – | 1210 | m/s |
| Mechanical loss coefficient (tan delta) | 0.0212 | – | 0.0235 | |
PA66 Molding Grade Absorption & permeability
| Water absorption @ 24 hrs | 0.62 | – | 1 | % |
| Water absorption @ sat | 7 | – | 9.3 | % |
| Humidity absorption @ sat | 2 | – | 2.7 | % |
| Water vapor transmission | 0.865 | – | 1.46 | g.mm/m².day |
| Permeability (O2) | 0.339 | – | 0.995 | cm³.mm/m².day.atm |
PA66 Molding Grade Processing properties
| Polymer injection molding | Excellent |
| Polymer extrusion | Limited use |
| Polymer thermoforming | Limited use |
| Linear mold shrinkage | 0.7 – 1.8 % |
| Melt temperature | 220 – 327 °C |
| Mold temperature | 40 – 80 °C |
| Molding pressure range | 6.88 – 172 MPa |
PA66 Molding Grade Durability
| Water (fresh) | Excellent |
| Water (salt) | Excellent |
| Weak acids | Unacceptable |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Acceptable |
| Organic solvents | Excellent |
| Oxidation at 500C | Unacceptable |
| UV radiation (sunlight) | Poor |
| Flammability | Slow-burning |