PA66 Lubricated 5% MoS2 Material Data Sheet

PA66 Lubricated 5% MoS2 (Polyamide 66) Material Data Sheet

PA66 Lubricated 5% MoS2 Overview

PA66 lubricated 5% MoS2 is a grade of polyamide 66 (PA66, nylon 66), designated Polyamide (Nylon) (Type 66, MoS2 Lubricated, Anti-friction). This PA66 lubricated 5% MoS2 material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PA66 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PA66 parts in-house and inspects them before shipment.

PA66 Lubricated 5% MoS2 Designation

Polyamide (Nylon) (Type 66, MoS2 Lubricated, Anti-friction)
TradenamesAlcom, Ashlene, Bestnyl, Chemlon, Clariant, Delta, Eplamid, Hifill, Hylon, Hyundai, Latilub, LNP Lubricomp, LNP Lubriloy, Lubemid, Lubricomp, Lubrione, Luvocom, Nilamid, Nymax, Nypol, Oxnilon, Plaslube, Plustek, Polynil, Pryme, Radici, Spartech, Terez, Torzen, Tribocomp, Trimid, Vydyne, Zytel

PA66 Lubricated 5% MoS2 Typical uses

Gears, cams, rollers, bearings, nuts and bolts, power tool housing, electrical connectors, combs, coil formers, fuel tanks for cars, kitchen utensils.

PA66 Lubricated 5% MoS2 Composition detail

Polymer95–96%
MoS2 (molybdenum disulfide)4–5%

PA66 Lubricated 5% MoS2 Physical properties

Density1.15–1.18g/cm3

PA66 Lubricated 5% MoS2 Mechanical properties

Young’s modulus1.54–1.91GPa
Specific stiffness1.32–1.64MN.m/kg
Yield strength (elastic limit)49–61.1MPa
Tensile strength53.4–65.3MPa
Specific strength42–52.5kN.m/kg
Elongation41–59% strain
Elongation at yield19–36% strain
Compressive modulus1.64–1.81GPa
Compressive strength67.7–74.8MPa
Flexural modulus1.59–1.91GPa
Flexural strength (modulus of rupture)60.1–73.4MPa
Shear modulus0.601–0.631GPa
Shear strength32.1–39.2MPa
Bulk modulus2.73–3.02GPa
Poisson’s ratio0.384–0.4 
Shape factor4.2
Hardness – Vickers16–17HV
Hardness – Rockwell M110–122 
Hardness – Rockwell R110–122 
Hardness – Shore D80–83 
Elastic stored energy (springs)693–1100kJ/m3
Fatigue strength at 10^7 cycles22.6–24.9MPa

PA66 Lubricated 5% MoS2 Impact & fracture properties

Fracture toughness3.42–3.77MPa.m0.5
Toughness (G)6.53–8.66kJ/m2
Impact strength, notched 23 °C4.3–5kJ/m2
Impact strength, notched -30 °C3.3–7.18kJ/m2
Impact strength, unnotched 23 °C50–107kJ/m2

PA66 Lubricated 5% MoS2 Thermal properties

Melting point249–265°C
Glass temperature54–66°C
Heat deflection temperature 0.45MPa202–221°C
Heat deflection temperature 1.8MPa88–127°C
Maximum service temperature90–130°C
Minimum service temperature-81–-71°C
Thermal conductivity0.282–0.293W/m.°C
Specific heat capacity1570–1630J/kg.°C
Thermal expansion coefficient111–116µstrain/°C
Thermal shock resistance242–327°C
Thermal distortion resistance0.00247–0.00261MW/m

PA66 Lubricated 5% MoS2 Electrical properties

Electrical resistivity2e17–5e18µohm.cm
Electrical conductivity3.45e-17–8.62e-16%IACS
Dielectric constant (relative permittivity)6.14–8.66 
Dissipation factor (dielectric loss tangent)0.0715–0.189 
Dielectric strength (dielectric breakdown)12.6–21.4MV/m
Comparative tracking index600  V

PA66 Lubricated 5% MoS2 Magnetic properties

Magnetic typeNon-magnetic

PA66 Lubricated 5% MoS2 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity1150–1280m/s
Mechanical loss coefficient (tan delta)0.019–0.021 

PA66 Lubricated 5% MoS2 Absorption & permeability

Water absorption @ 24 hrs0.6–0.98%
Water absorption @ sat6.7–8.9%
Humidity absorption @ sat2–2.6%

PA66 Lubricated 5% MoS2 Processing properties

Polymer injection moldingExcellent
Polymer extrusionLimited use
Polymer thermoformingLimited use
Linear mold shrinkage0.7 – 1.8 %
Melt temperature220 – 316 °C
Mold temperature50 – 80 °C
Molding pressure range34.4 – 172 MPa

PA66 Lubricated 5% MoS2 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisAcceptable
Organic solventsExcellent
Oxidation at 500CUnacceptable
UV radiation (sunlight)Poor
FlammabilitySlow-burning