17-4PH H1075 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)
17-4PH H1075 Stainless Steel Overview
17-4PH H1075 stainless steel is a martensitic precipitation hardening stainless steel (UNS S17400) in the wrought form. Condition: H1075 (Solution annealed; precipitation (age) hardened at 580°C; air cooled). This 17-4PH H1075 stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 17-4PH parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined 17-4PH parts in-house and inspects them before shipment.
17-4PH Designation
17-4PH, wrought
Condition
H1075 (Solution annealed; precipitation (age) hardened at 580°C; air cooled)
Processing of potentially corrosive liquids e.g. chemicals/oil/beverages/sewage, structural uses in corrosive environments, e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
356
–
553
MPa
17-4PH Impact & fracture properties
Fracture toughness
130
–
158
MPa.m0.5
Toughness (G)
83.8
–
123
kJ/m2
17-4PH H1075 Stainless Steel Thermal properties
Melting point
1400
–
1440
°C
Maximum service temperature
282
–
316
°C
Minimum service temperature
-73
–
-43
°C
Thermal conductivity
17.3
–
18.7
W/m.°C
Specific heat capacity
477
–
496
J/kg.°C
Thermal expansion coefficient
11.3
–
11.9
µstrain/°C
Thermal shock resistance
364
–
423
°C
Thermal distortion resistance
1.48
–
1.62
MW/m
Latent heat of fusion
260
–
285
kJ/kg
17-4PH Electrical properties
Electrical resistivity
75
–
85
µohm.cm
Electrical conductivity
2.03
–
2.3
%IACS
Galvanic potential
-0.19
–
-0.11
V
17-4PH Magnetic properties
Magnetic type
Magnetic
17-4PH Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5010
–
5140
m/s
Mechanical loss coefficient (tan delta)
3.1e-4
–
6.6e-4
17-4PH Processing properties
Metal casting
Unsuitable
Metal cold forming
Limited use
Metal hot forming
Acceptable
Metal press forming
Acceptable
Metal deep drawing
Unsuitable
Machining speed
13.7 m/min
Weldability Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIG
Good
Weldability – plasma
Good
Weldability – SAW
Not recommended
Weldability – TIG
Good
Brazeability
Good
Carbon equivalency
0.65 – 0.97
17-4PH Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Excellent
Strong acids
Acceptable
Weak alkalis
Excellent
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Excellent
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
Flammability
Non-flammable
17-4PH H1075 Stainless Steel Corrosion resistance
Pitting resistance equivalent number (PREN)
15 – 17.5
Pitting and crevice corrosion
Low (<20)
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Susceptible
Intergranular (weld line) corrosion
Good
Inorganic acids
Restricted
Organic acids
Moderate
Alkalis
Moderate
Humidity / water
Excellent
Sea water
Restricted
Sour oil and gas
Restricted
17-4PH Standards with similar compositions
Australia: 630 to AS 2837
China: 0Cr17Ni4Cu4Nb to GB 1220, 0Cr17Ni4Cu4Nb to GB 1221
France: Z4CNU17.4M to AFNOR NF A35-586, Z6CNU17.04 to AFNOR NF A35-581
Germany: 1.4542 to DIN EN 10088, X5CrNiCuNb16-4 to DIN EN 10088
Japan: SUS630 to JIS G4303, SUS630 to JIS G4304, SUS630 to JIS G4305, SUS630FB to JIS G4319, SUSF630 to JIS G3214
South Korea: STS 630 to KS D 3706, STS F 630 to KS D 4115, STS630 to KS D 3698, STS630 to KS D 3705, STS630FB to KS D 3691
USA: 17-4 PH to MIL-C-24111B, 5604 to AMS 5604, 5622 to AMS 5622, 5643 to AMS 5643P, 61 to ASTM A579, Grade F Class 1 to ASTM A1028, Grade F Class 1 to ASTM A982, IC-17-4 to MIL-S-81591, S17400 to ASTM A564/A564M, S17400 to ASTM A693, S17400 to ASTM A705/A705M-95, S17400 to ASTM A959, S17400 to ASTM F594, S17400 to ASTM F738M, S17400 to ASTM F836M, UNS S17400