17-4PH Cast H1100 Stainless Steel Material Data Sheet
17-4PH Cast H1100 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)
17-4PH Cast H1100 Overview
17-4PH cast H1100 is a martensitic precipitation hardening stainless steel (UNS S17400) in the cast form. Condition: H1100 – Solution treated and precipitation/age hardened at 1100°F (593°C). This 17-4PH cast H1100 material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 17-4PH castings from Turkey (Türkiye)? Modulus Metal supplies 17-4PH castings with in-house CNC machining and inspects them before shipment.
17-4PH Designation
17-4PH
Condition
H1100 – Solution treated and precipitation/age hardened at 1100°F (593°C)
Processing of potentially corrosive liquids e.g. chemicals/oil/beverages/sewage, structural uses in corrosive environments, e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes
17-4PH Cast H1100 Composition detail
Al (aluminum)
0
–
0.05
%
C (carbon)
0
–
0.06
%
Cr (chromium)
15.5
–
16.7
%
Cu (copper)
2.8
–
3.5
%
Fe (iron)
72.8
–
77.4
%
Mn (manganese)
0
–
0.7
%
N (nitrogen)
0
–
0.05
%
Nb (niobium)
0.15
–
0.4
%
Ni (nickel)
3.6
–
4.6
%
P (phosphorus)
0
–
0.025
%
S (sulfur)
0
–
0.025
%
Si (silicon)
0.5
–
1
%
Sn (tin)
0
–
0.02
%
Ta (tantalum)
0
–
0.05
%
17-4PH Physical properties
Density
7.82
–
7.9
g/cm3
17-4PH Cast H1100 Mechanical properties
Young’s modulus
197
–
207
GPa
Specific stiffness
25
–
26.4
MN.m/kg
Yield strength (elastic limit)
827
–
914
MPa
Tensile strength
896
–
990
MPa
Specific strength
105
–
116
kN.m/kg
Elongation
6
–
6.97
% strain
Compressive strength
910
–
1010
MPa
Flexural modulus
197
–
207
GPa
Flexural strength (modulus of rupture)
827
–
914
MPa
Shear modulus
88
–
92.5
GPa
Bulk modulus
142
–
150
GPa
Poisson’s ratio
0.27
–
0.281
Shape factor
27
Hardness – Vickers
250
–
460
HV
Elastic stored energy (springs)
1690
–
2070
kJ/m3
Fatigue strength at 10^7 cycles
364
–
542
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
357
–
552
MPa
17-4PH Impact & fracture properties
Fracture toughness
138
–
168
MPa.m0.5
Toughness (G)
94.6
–
139
kJ/m2
17-4PH Cast H1100 Thermal properties
Melting point
1400
–
1440
°C
Maximum service temperature
282
–
316
°C
Minimum service temperature
-73
–
-43
°C
Thermal conductivity
17.3
–
18.7
W/m.°C
Specific heat capacity
477
–
496
J/kg.°C
Thermal expansion coefficient
12.5
–
13.1
µstrain/°C
Thermal shock resistance
316
–
357
°C
Thermal distortion resistance
1.34
–
1.47
MW/m
Latent heat of fusion
260
–
285
kJ/kg
17-4PH Electrical properties
Electrical resistivity
75
–
85
µohm.cm
Electrical conductivity
2.03
–
2.3
%IACS
Galvanic potential
-0.2
–
-0.12
V
17-4PH Magnetic properties
Magnetic type
Magnetic
17-4PH Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5000
–
5130
m/s
Mechanical loss coefficient (tan delta)
3.1e-4
–
6.6e-4
17-4PH Processing properties
Metal casting
Limited use
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
14 m/min
Weldability Notes: Preheating is not required, post weld heat treatment is required
Good
Carbon equivalency
0.687 – 0.867
17-4PH Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Excellent
Strong acids
Acceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Excellent
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
Flammability
Non-flammable
17-4PH Cast H1100 Corrosion resistance
Pitting resistance equivalent number (PREN)
15.5 – 17.5
Pitting and crevice corrosion
Low (<20)
Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide