17-4PH H1025 Stainless Steel Material Data Sheet

17-4PH H1025 Stainless Steel Material Data Sheet (Martensitic, Precipitation Hardened)

17-4PH H1025 Stainless Steel Overview

17-4PH H1025 stainless steel is a martensitic precipitation hardening stainless steel (UNS S17400) in the wrought form. Condition: H1025 (Solution annealed; precipitation (age) hardened at 551°C; air cooled). This 17-4PH H1025 stainless steel material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 17-4PH parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined 17-4PH parts in-house and inspects them before shipment.

17-4PH Designation

17-4PH, wrought
ConditionH1025 (Solution annealed; precipitation (age) hardened at 551°C; air cooled)
UNS numberS17400
US nameASTM S17400, ASTM 61
EN nameX5CrNiCuNb17-4
EN number1.4542
GB (Chinese) name0Cr17Ni4Cu4Nb, 0Cr16Ni4Cu4Nb
JIS (Japanese) nameSUSF630, SUS630
Tradenames17-4 PH, AK Steel (USA); 17-4PH, Sandmeyer (USA); CATAMOLD 17-4PH, BASF (USA); AMS 5643 – 17/4 PH, Smiths (UK);

17-4PH Typical uses

Processing of potentially corrosive liquids e.g. chemicals/oil/beverages/sewage, structural uses in corrosive environments, e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes

17-4PH H1025 Stainless Steel Composition detail

C (carbon)0–0.07%
Cr (chromium)15–17.5%
Cu (copper)3–5%
Fe (iron)69.9–78.8%
Mn (manganese)0–1%
Nb (niobium)0.15–0.4%
Ni (nickel)3–5%
P (phosphorus)0–0.04%
S (sulfur)0–0.03%
Si (silicon)0–1%
Ta (tantalum)0–0.05%

17-4PH Physical properties

Density7.79–7.87g/cm3

17-4PH H1025 Stainless Steel Mechanical properties

Young’s modulus197–207GPa
Specific stiffness25.1–26.5MN.m/kg
Yield strength (elastic limit)1000–1110MPa
Tensile strength1070–1180MPa
Specific strength128–141kN.m/kg
Elongation14.8–17.2% strain
Compressive strength958–1290MPa
Flexural modulus197–207GPa
Flexural strength (modulus of rupture)1000–1110MPa
Shear modulus77–80.9GPa
Bulk modulus142–150GPa
Poisson’s ratio0.27–0.281 
Shape factor22
Hardness – Vickers250–460HV
Hardness – Rockwell B109–112HRB
Hardness – Rockwell C36–41HRC
Hardness – Brinell334–370HB
Elastic stored energy (springs)2470–3030kJ/m3
Fatigue strength at 10^7 cycles364–542MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
357–552MPa

17-4PH Impact & fracture properties

Fracture toughness116–142MPa.m0.5
Toughness (G)67.3–98.9kJ/m2

17-4PH H1025 Stainless Steel Thermal properties

Melting point1400–1440°C
Maximum service temperature282–316°C
Minimum service temperature-73–-43°C
Thermal conductivity17.3–18.7W/m.°C
Specific heat capacity477–496J/kg.°C
Thermal expansion coefficient12.5–13.1µstrain/°C
Thermal shock resistance382–432°C
Thermal distortion resistance1.34–1.47MW/m
Latent heat of fusion260–285kJ/kg

17-4PH Electrical properties

Electrical resistivity75–85µohm.cm
Electrical conductivity2.03–2.3%IACS
Galvanic potential-0.19–-0.11V

17-4PH Magnetic properties

Magnetic typeMagnetic

17-4PH Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5010–5140m/s
Mechanical loss coefficient (tan delta)3.1e-4–6.6e-4 

17-4PH Processing properties

Metal castingUnsuitable
Metal cold formingLimited use
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingUnsuitable
Machining speed13.4 m/min
Weldability
Notes: Preheating is not required, post weld heat treatment is required
Good
Weldability – MIGGood
Weldability – plasmaGood
Weldability – SAWNot recommended
Weldability – TIGGood
BrazeabilityGood
Carbon equivalency0.65 – 0.97

17-4PH Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsExcellent
Strong acidsAcceptable
Weak alkalisExcellent
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CExcellent
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

17-4PH H1025 Stainless Steel Corrosion resistance

Pitting resistance equivalent number (PREN)15 – 17.5
Pitting and crevice corrosionLow (<20)
Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Hydrogen sulfide
Susceptible
Intergranular (weld line) corrosionGood
Inorganic acidsRestricted
Organic acidsModerate
AlkalisModerate
Humidity / waterExcellent
Sea waterRestricted
Sour oil and gasRestricted

17-4PH Standards with similar compositions

Australia: 630 to AS 2837
China: 0Cr17Ni4Cu4Nb to GB 1220, 0Cr17Ni4Cu4Nb to GB 1221
France: Z4CNU17.4M to AFNOR NF A35-586, Z6CNU17.04 to AFNOR NF A35-581
Germany: 1.4542 to DIN EN 10088, X5CrNiCuNb16-4 to DIN EN 10088
Japan: SUS630 to JIS G4303, SUS630 to JIS G4304, SUS630 to JIS G4305, SUS630FB to JIS G4319, SUSF630 to JIS G3214
South Korea: STS 630 to KS D 3706, STS F 630 to KS D 4115, STS630 to KS D 3698, STS630 to KS D 3705, STS630FB to KS D 3691
USA: 17-4 PH to MIL-C-24111B, 5604 to AMS 5604, 5622 to AMS 5622, 5643 to AMS 5643P, 61 to ASTM A579, Grade F Class 1 to ASTM A1028, Grade F Class 1 to ASTM A982, IC-17-4 to MIL-S-81591, S17400 to ASTM A564/A564M, S17400 to ASTM A693, S17400 to ASTM A705/A705M-95, S17400 to ASTM A959, S17400 to ASTM F594, S17400 to ASTM F738M, S17400 to ASTM F836M, UNS S17400
Tradenames: AL 17-4 PRECIPITATION HARDENING ALLOY, AL17-4 PRECIPITATION HARDENING, CRUCIBLE 17 CR-4 NI, DOMINIAL RAS-CU, EAGLE & GLOBE 630, KRUPP WL 1.4548, NIROSTA 4542, NIROSTA 4548, SLATER TYPE 17-4, UNILOY 17-4